AN OUTLINE HISTORY OF CONSERVATION IN ARCHAEOLOGY AND ANTHROPOLOGY AS PRESENTED THROUGH ITS PUBLICATIONS
Niccolo Leo Caldararo
ABSTRACT—The article provides a survey of the historical development of preservation practice in archaeology and anthropology, with reference to both techniques and philosophy. The primary focus is placed on the evolution of a body of knowledge through the literature and the rise of scientific methods and specialization. The article includes a substantial historical bibliography.
1 EARLY DEVELOPMENTS IN ARCHAEOLOGICAL AND ANTHROPOLOGICAL CONSERVATION
This paper will discuss briefly some of the historical origins of conservation in archaeology and anthropology; it will, however, focus mainly on archaeology. Although conservation treatments applied by conservators and restorers in general to archaeological and anthropological artifacts have not developed separately from conservation efforts in anthropology and archaeology, they generally represent two different trends of thought and practice which have influenced each other.
The earliest restorations were done in the classical workshops of craftsmen and artists of every great civilization. For example, Ku-Szu-Ksieh (Van Gulik, 1958) described methods of repair for paper scrolls in fifth-century A.D. China. The transition from these origins to the modern professional concept of conservation is of particular interest to the field of archaeological and anthropological conservation. Nevertheless, the roots of scientific conservation were traced by Gettens (1974) only to the Rome Conference of 1930, sponsored by the League of Nations. Santucci (1963), however, began his history with chemical experiments by Chaptal on restorative methods for paper, parchment, and papyrus reported in 1787, and the 1809 report, also by Chaptal, on ancient pigments; Christoforno Marino's nineteenth-century work on the restoration of faded writing on parchment (Gallo, 1951); and Piaggi and Davy's experiments with unrolling papyrus from Herculaneum (Bennett 1806; Davy, 1821).
The tragedies which befell antiquities found in Herculaneum, Pompeii, and Stabia at the hands of restorers certainly influenced the scholars and scientists of the period of their discovery (Winckelman, 1771).1 The desire to see objects in their original condition, unaltered by additions, and to detect fakes led to scientific procedures. This desire, along with the need to establish provenance of manufacture and to develop systematic criteria to resolve questions of the objects' materials and techniques led to the introduction of the chemical analysis of ancient objects first published2 by M. H. Klaproth in 1798 (Goffer, 1980).
Analysis of excavated metals, chiefly bronzes, advanced rapidly between 1800 and 1875 with the publication of twenty-five papers by 1850 and many more by 1875 (Caley, 1951). One student of conservation history credits archaeological research with establishing the philosophy of preserving original creations and ending the restorative destruction of the sixteenth to nineteenth centuries (Hulmer, 1955:72). Whether this philosophy can be credited with a similar change in attitude toward archival materials, books, maps, etc., is unclear, nevertheless the impetus toward the preservation of such materials also appeared at this time.
Scientific studies on the effects of gas lights on leather bindings were made by Faraday in 1843, by G. Davis in 1877, and by C. Woodward in 1888. The first attempts to apply practical experience and scientific knowledge in restoration were published by Bonnardot in 1846 and 1858. The application of techniques from various disciplines and communication between scholars and scientists on preservation problems were pioneered by Cardinal Ehrle, keeper of the Vatican Library and promoter of the International Conference of St. Gallo on preservation of archival materials in 1898 (Santucci, 1963:40).
The St. Gallo Conference was held at the same time that the first report of the Committee on the Deterioration of Paper appeared in London. It was followed by the Archivists' Conference in Dresden in 1899, the International Congress of Libraries in Paris in 1900, and the establishment of a scientific committee for the study of the decay of leather bookbindings by the London Society for the Encouragement of Arts, Manufacture and Commerce in 1900. A similar committee was created in Germany in 1911, and the foundation of the restoration laboratory of the Rome Archivio Centrale dello Stato occurred the same year.
2 EARLY TWENTIETH-CENTURY ORGANIZATION OF THE FIELD
Especially important were discussions and cooperative efforts which resulted from the Cairo (1937), Athens (1931), and Madrid (1934) conferences of scientists and scholars and representatives of the international museums sponsored by the International Museums Office of the League of Nations (IMO, 1949), which established the necessity for close inter-relations between excavation and museum work. Much of this work is being investigated anew today with special focus on ancillary problems to ensure the proper care of artifacts, such as cataloguing, documentation and reporting (cf. King, et al. in Curator, 21/1, 1980), site or field conservation, and selection of criteria for collecting and storage (McGimsey and Davis, 1977; Grosso, 1978; Adamson, 1979; Lindsay Jr., 1979). Standards for proper treatment, including documentation, in the field and the laboratory can increase the percentage of artifacts successfully retrieved and susceptible to productive long-term study (Feilden, 1979:34; 1982). The need in practice for such proper care has been reiterated for several years by various authors (Ford, 1977; Marquardt, et al., 1977; Frere, et al., 1978; Davies, 1978; Christenson, 1980; Lindsay Jr., 1979; Bourque, Brooke, Kelly and Morris, 1980; Stanley-Price, 19843
Of course, the recovery of artifacts was of primary importance in the early phases of the history of archaeology. What was called excavation often resulted in not only the loss of critical data on the relationship between the object and stratigraphy but also the mass destruction of sites by a whole scale removal as well as the loss of large numbers ofobjects by theft, inadequate supervision and poor recovery techniques. This was often due to a lack of understanding of the relationship between the object and its environment but more often due to the disorder inherent in much if not most archaeological work in the nineteenth century (Hole & Heizer, 1965; Wheeler, 1954). The development of conservation techniques in archaeology has seen as uneven an evolution as has the excavation report (Caldararo, 1984) and in many ways suffers the same vagaries in application due to lack of priority and a lack of funding.
The Lindsay study (1979:127–30) found that the care of collections was at best a secondary consideration in the process of archaeological collection. Storage and conservation were seldom addressed in reports and when they were they reflected a considerable diversity of treatment. The report in general found a lack of commitment to care of collections and proper storage and especially to the conservation of collections. This lack of concern, however, may be a result of a lack of funding as well as access to information. In a survey of thirty-seven course offerings by anthropology departments in American colleges and universities, conservation or preservation was mentioned in only fifteen course descriptions from ten institutions.4
3 INITIAL WORKS
The specifics of a history of archaeological and anthropological conservation remain vague and only fitfully illuminated in the literature. Although some archaeologists have written notes on the conservation and restoration techniques which they applied in the field and laboratory, the great majority have not. Fewer still have included these notes in their reports. One of the few sources of such information is the Society for American Archaeology Notebook (SAA-N). This informal publication issued from 1939 to late 1942 provided a forum for archaeologists to describe new treatments in the field and museum lab and to ponder common problems. Museum Work, published by the American Association of Museums, Curator, and Museum News in America, and the Museums Journal in England, have provided a similar outlet for archaeologists and anthropologists in museum settings. In 1933 the Fogg Museum began the publication of a periodical of a scientific approach as applied to art and archaeology, Technical Studies in the Field of the Fine Arts.
Of the publications pertaining to artifact conservation, it is remarkable to note the similarity in organization and subjects covered they reveal on comparison. Some similarity is due to the nature of the objects studied. From Rathgen (1905) to Dowman (1970) knowledge of the environment, soil conditions, changes in conditions which an object would go through, and an awareness of the limitations of the available materials for treatment have been a consistent thread.
The first two works5 detailing the use of scientific techniques applied to the restoration and conservation of artifacts appeared in Germany just before the turn of the twentieth century. They were produced in response to the need to preserve objects of Egyptian origin in Northern European museums. The publication by Voss, appearing in 1888, was prepared at the request of the German government (Rathgen, 1905, ed.:v). Rathgen's work was published in German and then translated into English in 1905 (Otto, 1979:47). It stands out from the general literature of conservation in that it was more of a critical summary of the work of European conservators and scientists with whom he and Voss corresponded and whose work they knew through reports in publications and of the experiences of collectors as well. Generally, Rathgen outlined the works of others and criticized it in terms of his own and colleagues' work. Both books may be said to have resulted from problems produced by the extensive collecting of artifacts in Egypt by Lepsius and other German archaeologists in the nineteenth century. The work of Voss and Rathgen has been carried on by German conservators publishing their results in the pages of Der Präparator and Maltechnick-Restauro and other publications.
In the United Kingdom, Alexander Scott published three reports in 1921, 1923, and 1926 on treatments done in the British Museum. Lucas published a comprehensive text of his conservation treatments in its original form in 1924, the result of his work on the artifacts from the Tomb of Tutankh-Amen and his earlier studies as the Director of the Egyptian Chemical Department (Anon., 1924). At about the same time he set up a laboratory at the Museum of Antiquities in Cairo. The impact of this European work on American archaeologists and museum workers came with the publication of Douglas Leechman's [application of Lucas's and other European practitioners'] techniques and procedures to the conservation of North American artifacts (1931). Leechman explains in his introduction that, at the time, there were only three books on the subject of preservation of museum specimens that were of any use and that one of these was the “out-of-date” translation of Rathgen. He states that the three were principally concerned with archaeological materials, particularly those from Egypt.
Much of Leechman's philosophy and methodological procedure6 in conservation has stood the test of time, with the exception of some vague introductory phrases in which he cautions against changing the appearance of an object “…except, in some cases, very much for the better,” and promotes cleaning to return a specimen to “…the condition in which its original owner or maker would have kept it.” Even if we had ethnographic information detailed enough to tell us in every case how a “typical” owner might keep a particular artifact, by modern professional standards returning it to this state would be a questionable and subjective exercise. Artifacts are found (i.e. collected from living users or archaeologically) containing traces of food, showing wear, or possessing examples of repairs done in aboriginal settings which provide information about the people, their technology, diet and the attitudes they held toward the artifacts.
Conservators are often faced with the problem of determining what is an aboriginal repair and what is a repair executed by a collector or dealer. Fried (1981:229–45) has discussed this problem in detail as it affects scholarship. We have also some to realize since Leechman's time, that “cleaned” and “restored” or “conserved” have further implications which can compromise the objects conceptually (Wolf & Mibach, 1983).
This is especially a problem with museum objects7 where articles of use, practical or spiritual, may be transformed into (isolated into) objects for aesthetic contemplation only. With archaeological materials, we have the added problem of the possible compromise of analysis, where the potential for trace element analysis and dating can be altered or destroyed even by simple washing and handling (Brothwell, 1965; Geidel, 1982; Loy, 1983; Janaway, 1983). An excellent example of the dangers involved is the case in which Colin Fink cleaned an Egyptian Old Kingdom ewer and basin by electrolytic reduction and then decided after his examination of the objects that the Egyptians had had a chemical method of plating antimony on copper (1934). Forbes (1950:264) pointed out after a subsequent analysis that the antimony plating was due to the electrolytic reduction of the copper objects by Fink.
In the 1930s the series of conferences sponsored by the International Office of Museums (IMO) brought together archaeologists, scientists and scholars from all over the world. At these conferences discussions of archaeological excavation, restoration and museology, and a desire to standardize practice led to several publications. A journal, Mouseion, published by the IMO allowed results of work to be spread to colleagues who could not meet. Another IMO publication which resulted from conference discussions was the Manual on the Technique of Archaeological Excavations (1940). Among the members of the editorial committee which produced the Manual was H. J. Plenderleith, then Professor of Chemistry, Royal Academy of Arts, and Keeper of the Research Laboratory at the British Museum, London. The Manual was planned as a standardized guide to excavation work anywhere in the world. It contained a chapter on field conservation which drew on the recently published works of Plenderleith (1934), Rosenberg (1934), Sana Ullah (1934)S and that earlier of Rhoussopoulos (1911–12), among others.
Plenderleith published a summary of his work (1956) which he intended as a handbook or workshop guide much like the works which had preceded it (Rathgen, Lucas, etc.). The book, revised with the help of Werner in 1971, has been of immense importance in both the general field of conservation and in archaeology. Their work, like that of those who preceded them, was directed at introducing scientific methodology into a field which had previously been dominated by craftsmen. Both Plenderleith's 1956 edition, and his 1971 edition produced with Werner, are major contributions to the field of conservation and touch on field conservation techniques. Both editions are generally concerned with treatments of objects once they are in the museum. Some archaeological conservators have criticised their lack of detail in certain areas, for example Hodges (1975:37); with respect to ceramics.
4 SCIENTIFIC METHODOLOGY AND CONSERVATION IN ARCHAEOLOGY AND ANTHROPOLOGY
The first American publication relating to archaeological and anthropological conservation was Forrest E. Clements's article in American Antiquity in 1936 (excepting the brief instructions of Holmes and Mason, 1902). It was basically a summary of Leechman's earlier work in the context of Clements's own experience. It was not until Keel published his work in 1964 that American archaeology had a comprehensive manual designed especially for American collections in museum and university storage conditions. Still, Keel, like Leechman, dealt mainly with museum artifacts. His work was inspired by Plenderleith's 1956 edition of The Conservation of Antiquities and Works of Art to which he devotes almost the entirety of his introduction, summarizing the earlier publication.
With the introduction of scientific methodology, emerging technology of the day was quickly applied to pressing problems which threatened disastrous results if unchecked (e.g. see Howie, 1984). For example, Leechman advised the use of celluloid dissolved in acetone as a consolidant for a wide variety of materials. He also sprayed gasoline on artifacts to fumigate them (Leechman, 1931:129, and passim). However, this new tendency toward general use of chemical treatments was questioned quite early by Gettens (1933:41-1), who suggested that Lucas's use of celluloid solution and paraffin was inappropriate for some objects.
In the last 20 years we have seen a vast array of synthetic products utilized for conservation and restoration. A rather informal process of introduction developed8 as the discipline of conservation matured. Rapid aging tests were occasionally applied prior to general introduction. Yet as time has passed it has become evident that the aging of these treatments in real time and the effects of varying conditions may produce unexpected results.9 In this vein we have the recent problems upon aging developed by soluble nylon (Sease, 1981) and the effect of light on plastics and thermoplastics in particular (Lightbody and Roberts, 1954; Pappas and Winslow, 1981).
It is certain that, since the founding of the Institute of Archaeology by Sir Mortimer Wheeler in 1937 at the University of London, scientific attitudes have greatly aided the archaeologist in site retrieval of artifacts and in laboratory procedures for their preservation. This has become most apparent in underwater and marine archaeology, where retrieval is increasingly dependent on systems developed by conservators (Bourque, Brooke, Kelly and Morris, 1980). Recent literature contains examples of archaeologists who recognize the need for and utility of the expertise of conservators (South, 1976), though Clark (1954) and Wheeler (1954) set early foundations.
Perhaps the bulk of innovations in technology along with new materials applied to archaeological retrieval and laboratory work occurred without the intervention of conservators over the last 200 years. This process was generally haphazard and makeshift, with treatments applied with whatever materials were handy and without prior experiment on long-term effects, which often resulted in disastrous losses (e.g. Wheeler, 1954: 168). It is obvious, however, from the published literature of conservation scientists, researchers of the British Museum and the Institute of Archaeology, as well as that of archaeologists, that many innovations were introduced either by way of scientific experimentation and practice applied in museums or through collaboration of conservators, archaeologists, and consulted scientists (cf. Plenderleith and Werner, 1971 ed.; Organ, 1968; McCawley, 1977; Howie, 1984).
The archaeologist often requires microanalysis of materials for chemical content or trace elements, etc., and has historically gone to the research scientists of the museum conservation laboratories (as well as to university scientists) for aid (e.g. Gettens, 1933). At this point the scientist is engaged in archaeometry. Archaeologists have learned much about ancient technologies by the detailed analysis of artifacts and their components. This process of analysis when uncovering the materials used as well as the techniques of manufacture can involve restoration of the object (Woolley, 1934:70). (Previously, reconstruction had been done either by archaeologists, departmental employees, graduate students, or by specialized museum craftsmen called preparators, the “Jimmy Valentines” of science as Stucker (1977:201) describes their paleontological counterparts, who often executed the exhibition of objects.)
5 MODERN DEVELOPMENTS AND PRACTICE
With the application of new scientific techniques and procedures, new information can be discovered about formerly restored artifacts (Scott, 1926: 39–40; Greene, 1979). To this end the teaching of archaeological conservation at the Institute of Archaeology of London University has been likened to that of a physician's education: the practitioner must make a diagnosis of an object's condition and propose treatment (Gedye & Hodges, 1964: 84–7). However, given the above context, both student and archaeologist will encounter some difficulty in acquiring information concerning past and present conservation treatments and procedures. Although the Art and Archaeology Technical Abstracts cross-reference published articles relating to conservation, the amount of information in print on archaeological and anthropological conservation is comparatively small in relation to other fields of conservation or the body of anthropological literature.
With the rapid increase in technological apparatus and complex analytical procedures in archaeometry and conservation, specialist scientists have become more prevalent. As Werner turned more toward ethnographic conservation, especially that of fragile organic objects, another scientist at the Research Laboratory, Robert M. Organ, began specializing in treatment and storage of metals and wood.10 Organ published the practical but highly technical Design for Scientific Conservation of Antiquities in 1968. Garry Thomson, scientific advisor to the National Gallery, London, came to specialize in environmental concerns in museums, (such as air conditioning and the effects of air pollution on works of art). His 1978 publication, The Museum Environment, is a concise description of environmental problems, their causes and prevention. W. A. Oddy, another British Museum Research Laboratory scientist, concentrated his studies on metals and stone: corrosion and deterioration prevention and treatment (e.g. Oddy & Hughes, 1970; Oddy, 1977).
A similar trend has developed among continental European conservation scientists. The French11 had been filling the pages of Mouseion from its inception, as well as Studies in Conservation(France-Lord, 1962; Weil, 1958) with detailed reports of their work, most notably in the conservation and analysis of archaeological metals. Italian contributions ranged from site prospecting (Lerici, 1961) to the treatment of wooden objects (Augusti, 1959) to Torraca's substantial aid to the field in the application of solvents to problems in conservation (Torraca, 1975). In Poland, Jedrzejewska (1962; 1963–64) and in Czechoslovakia, Pelikan (1964; 1966) reported on progress in the treatment of archaeological artifacts, especially metals.
Other European scientists in collaboration have published works on specific subjects. An example is the work by Mühlethaler, a Swiss Scientist, Bachman, (Swedish), and Noack (German), Conservation of Waterlogged Wood and Wet Leather, published in 1973. Mühlethaler also produced a comprehensive text on conservation (1967), while Stambolov published a major work on the methods of preparation and restoration of skin objects (1969) from his Amsterdam laboratory. Significant research and experimentation were undertaken in Scandinavia. In the area of textile conservation, the first conservation studio conceived to operate under “scholarly control” was organized by two Stockholm museum directors under the leadership of Agnes Branting in 1908. Here scientific research and analysis were applied to the conservation of all types of textiles, in cluding archaeological textiles (Geijer & Franzen, 1975:7). Excavation of archaeological shipwrecks such as the “Wasa” and a long list of other excavated wrecks by Scandinavian conservators and archaeologists developed conservation techniques on a wide range of objects (Patoharju, 1975:183–187;Rosenqvist, 1959). Finally, Christensen (1952;1956) made substantial advances in the conservation of water-logged wood in Denmark.
The subject of conservation in excavation was never the subject of a comprehensive work, although Plenderleith's chapter in the IMO Manual (1940) was an early yet brief attempt. This may, however, reflect the youth of the field of conservation, as there have been few generally accepted text books produced as opposed to those available in an older discipline such as archaeology, no less technical or complex, which has a wide selection of up-to-date basic texts produced regularly. Dowman's Conservation in Field Archaeology, published in 1970, was as Oddy (1973:44) stated, “ …the first (work) to describe in simple form, treatments which may safely be carried out on archaeological finds in the field.” Dowman's work is an excellent compendium of field techniques, treatments both for rescue operations and field laboratories as well as storage directions and therefore a partial exception to the above generalization, extending care into the museum or university laboratory. For Dowman, aside from being out of print and containing some poor science (Oddy, 1973:45), has provided a much needed focus on materials, conditions, soils and methods of treatment specifically for the archaeologist. Some of Dowman's deficiencies are covered in a 1984 IC-CROM publication edited by Stanley-Price (1984), but although it includes many references, this publication fails to address other areas such as the role of conservation in post-excavation analysis.
A number of archaeological textbooks contain chapters or short sections which describe in more or less detail the authors' practices in the field and laboratory with regard to conservation (e.g. Wheeler, 1954; Brennen, 1973: 151 and 161; Robbins, 1965: 173;88). Most of these are simply outlines of practice or lists of suggested procedures, chemicals and apparatus. Both of Heizer's Guides fall into this category (Heizer, 1958; Heizer and Graham, 1967). The best of these texts give examples of procedures with lists of materials as well as some cautionary remarks and suggested alternatives, developed in some detail, differing from the former group in the specifics provided and the background sketched to help deter possible problems. Examples of these are Hume 1968 and Joukowsky, 1980. With the exception of Joukowsky, none of these provides a thorough reading list or bibliography upon conservation. None presents a conservation paradigm in a manner as complete as a workbook or a descriptive narrative as does Dowman, 1970.
A recent article by Katherine R. Singley (1981) falls between Joukowsky and Dowman in descriptive effectiveness of directives. It is an excellent outline of what should be done in the field for the care of artifacts after excavation. “Outline” must be stressed, for this is a very brief work; useful as this paper is it does not touch on ecofactual remains, which make up a large part of many collections and excavation materials.
Rescue publications of the Department of Archaeology of the University of Southhampton, especially Leigh (1978), give clear directions for field work but are generally limited to packing and storage. There are also several articles by Australians on conservation. Ambrose (1968) produced a practical summary of field conditions in Australia and appropriate treatments, and McCarthy (1970) edited a volume containing several works on a variety of problems.
Although there are professional guidelines in the field of conservation (AIC, 1980), there is no standard view of treatment in every case. There is a wide variation in what is regarded as the proper treatment for any particular object or whether there should be any treatment at all (Beck, 1982). Plenderleith admonished in 1940 (IMO, 1940:143), that the archaeologist must not leave objects in the hands of the conservator and give him carte blanche. The archaeologist must have a clear understanding of what can be done in the field, with those items left in situ as well as those recovered, and what can be treated in the museum or university laboratory. In practice, the archaeologist should have specific objectives which will dictate the type of conservation. However, in my experience these objectives are often short-sighted with respect to the survival of the majority of objects, and the most often described treatments are cosmetic or are so concerned with the immediate survival of the object for analysis that long-term treatments for survivability cannot be assured.
Communication between archaeologist and conservator must be an ongoing process to update what works in the field and to clarify the long-term effects of all treatments including those that may hinder research or analysis. Research and experimentation must be facilitated for the successful recovery and preservation of artifacts.
The retrieval of fragile fragments or of impressions of objects and the detection of trace elements or information concerning the former existence of structures or objects (Biek, 1963:60–65) is the meridian between the role of the conservator and that of the analytical scientist. Still, with all the technical skill of the scientists and the increasing specialization among conservators, it is the training of the excavators which is of utmost importance. It is with their ability and awareness that the successful recovery of an object begins.
For historical collections one may also mention Guldbeck (1972), published by the American Association for State and Local History, Waterer's 1972 work on leather which touches on archaeological and ethnographic materials, and Lewis's Manual for Museums (1976) which contains information derived from the work of the United States National Park Service centralized laboratories set up in the 1930s by Carl P. Russell. While most of the efforts of these laboratories have been oriented toward storage and exhibition as it is reflected in the content of this volume, there has been a long tradition of preservation treatments established by Park Service workers. Lewis's work follows on that by Ned J. Burns (1941); both were written for curators, to provide guidance to practical solutions for collections. The impact of Burns's work, however, is problematic as even Keel (1963) hardly mentions Burns's work and then only that concerning the treatment of skin. Nevertheless, Burns's work was very detailed and his audience, being the Park Service personnel under whose care were many thousands of objects, probably gave his suggestions on treatments and care a very wide application. However, with reference to this skin material, the work of Burns and that of Waterer mentioned above are of less value to archaeologists and anthropologists than the comprehensive work of Reed (1972).
Rowe (1953), in his summary of technical aids in anthropology mentions Rathgen (1905), Rosenberg (1917), Plenderleith (1934) and Leechman (1931) as the comprehensive texts in restoration. He mentions Lucas (1924) for chemical identification and analysis and Gettens (1950) and Fink (1933) for specific applications. The appearance of an article such as that by Velich (1965) in a journal of the professional caliber of Curator perhaps belies the actual effect of much of this work described above. While Velich's description of his treatments of skin artifacts of American Indians were not entirely unacceptable in the context of the time, they are extremely pedestrian in retrospect and must indicate a lack of familiarity with earlier published work, most specifically in his restorative efforts with ballpoint pen.
6 SPECIFIC GEOGRAPHIC DEVELOPMENTS
To return to Canadian archaeology, passed over after the discussion of Leechman's early contribution, it has had a rapid and intense involvement with conservation. William Todd, Chief Conservator of the Royal Ontario Museum until his death in 1963, published several papers on the conservation of materials, his subjects ranging from bone preservation (1941) to restoration of Chinese grave figurines (1952) to preservation research in Chinese bronzes. In 1966 the British Columbian Provincial Museum recruited its first conservator, who was the only one west of Toronto for the next four years (Ward, 1978:9). Care of collections prior to this date had been executed by other staff specialists. In 1970 the first course in conservation was established at the University of Victoria, entitled “Conservation of Antiquities,” as a course for curators. The Canadian Conservation Institute (CCI) was originally conceived in 1972 at Ottawa and two centers were established in 1974, the Pacific Regional Center and an Atlantic Regional Center, followed by a small facility in Quebec in 1977, with Erika Schaffer the principal scientist involved in the preservation research program for archaeological and anthropological materials of the CCI. Her work as a conservation scientist both in identifying materials of composite artifacts and designing treatment procedures has added considerably to the development of an organized methodology (1971, 1974, 1976, 1981), as has the work of another Canadian scientist, Mary-Lou Florian (1976, 1977, 1978, 1981). The development in Canada of the application of scientific techniques in archaeological conservation has been rapid especially in wet site and frozen site problems (Hett, 1978). Mac-Donald presents a concise outline of the development of wet site archaeology in Europe and North America in his 1977 article.
While conservation in Australia dates well into the last century with the establishment of a general lab in New South Wales (Lloyd, 1981), conservation work there has benefited from conservators with a broad range of skills and interests from fine arts to archaeology. One example is Boustead, who treated a wide range of ethnographic objects (Boustead, 1960; 1966). Australian archaeologists have written several articles on both field practice and museum work (e.g. Macintosh, 1968; McCarthy, 1970). Their publications in general reflect a close relationship with European (especially British) conservation efforts as well as local experimentation. Boustead, like many Australian conservators, learned his trade as an apprentice and later augmented his skills by tours of study in Europe, mainly England. Many Australian cultural institutions provided training for other surrounding nations through funds provided by the Commonwealth; these ranged from India to Pacific Island nations.
The tradition of the independent efforts of museum preparators in setting up conservation facilities is seen in the creation of the first conservation lab in New Zealand in 1953 (Thompson, 1985). The Pacific Regional Center, at its Honolulu facility in Hawaii, has trained local residents and treated regional collections from the Pacific Islands, as well as sent conservators out on location (Lee, 1978). The Pacific Regional Center resulted from a study undertaken by Werner in 1973 and sponsored by the Bishop Museum to determine the needs of Pacific Region museum institutions which led to the establishment of the Pacific Center in 1974 (UNESCO, 1980).
The Soviets and East Europeans developed parallel technology in the application of materials and have conducted extensive research and experimentation with synthetics (Nogid & Rozdnyak, 1965; Tomashevich, 1969). Grabar published a restoration manual in 1960 which presents a mixture of synthetic (new) and old traditional methods with some criticism of the poor aging results of some particular traditional methods (Kovostovetz and Thomson, 1963). The same can be said of the Japanese (Higuchi and Aoki, 1976; Aoki, 1985).
Concerning the Japanese, Yamasaki (1957:83) places the first technical conservation work in 1919 with the government-formed committee on the wall paintings of the Horyuji temple at Nara. An attempt to stabilize the peeling paint was undertaken using natural resins (copal), but the trial in a small area failed to produce satisfactory results and was discontinued. In 1933 Professor S. Taki of Tokyo University organized a small study group of art historians, physicists, chemists, biologists and architects. Discussions of methods of repair and conservation of art objects and studies of scientific and new methods of repair compared to traditional methods were undertaken. In 1947 the group was organized into the “Association of Scientific Research in Antiques” with Professor Y. Shibata as president. A journal was established by this group, Scientific Papers on Japanese Antiques and Art Crafts, the first issue appearing in 1951, although today the primary Japanese publication for conservation is Science for Conservation.
In addition to these efforts, the Institute of Art Research in Tokyo, founded in 1930, was reorganized in 1952 as the Tokyo National Research Institute of Cultural Properties, with a Department of Conservation added to it (Yamasaki, 1957:83). This Department of Conservation was housed in the Tokyo National Museum and was concerned mainly with the conservation of paintings and sculptures in temples and museums. This Department of Conservation was later changed to the Department of Conservation Science and a Department of Restoration Techniques was added (Ito, 1979:xi).
In 1902 the Archaeological Survey of India proposed a chemical branch, which was established in 1917 when a laboratory was set up in the Indian Museum in Calcutta. Later the laboratory was transferred to Dehre Dun and work organized on methods established at the British Museum Laboratory (Swarnakamal, 1975:25). A laboratory was set up at the National Museum, New Delhi, in 1958 as a central major research facility (Gairola, 1960; Agrawal, 1963). T. R. Gairola, Chemist, National Museum of India, New Delhi, published a Handbook of Chemical Conservation in 1960 which offered recommendations for treatments of all types of objects found in Indian museums; the handbook is organized by physical composition (organic, metals and siliceous). Basically it is a manual for museum workers, written for the post-graduate students of the Department of Museology of the University of Baroda, although it does contain examples of treatments of archaeological materials. Gairola draws heavily from the European and American literature and his own extensive experience.
Shortly after the establishment of a central conservation laboratory at the Baroda Museum for the State of Gujarat, Swarnakamal published a book, Protection and Conservation of Museum Collections (1975), which is entirely concerned with treatments in museums. Individual treatments of archaeological materials were from time to time published in several Indian journals including Journal of Indian Museums, and Ancient India. Other Indian conservation laboratories were established at Lucknow, and at the National Museum, New Delhi. In 1977, O. P. Agrawal, who studied under Gairola as well as at the Instituto Centrale del Restauro in Rome, published a book on the Care and Preservation of Museum Objects, one of a series of books on conservation in Indian museums and in Southeast Asia; it includes a bibliography on conservation in India. Agrawal is the Director of the National Research Laboratory for Conservation of Cultural Property, Lucknow, and has edited a journal, Conservation of Cultural Property in India, from 1967 to the present. He produced several studies on the conservation needs of Asian nations as well as edited several books, including Conservation in the Tropics (1973), Documentation in Museums (1974) and The Small Museum (1975). His survey of conservation needs and techniques of Southeast Asian cultural properties, originally published in Museum in 1975 as Conservation in South and Southeast Asia, was expanded and republished by Butterworths in 1984.
In Africa, archaeological and anthropological conservation has been derived in most part from European efforts, particularly British and French. A manual for conservation of collections of Middle African museums was produced by Kennedy in 1959 and contains the usual organization, beginning with the effects of climate on objects, the agents of deterioration (insects, microorganisms, etc.) and then an overview of restoration techniques. A substantial number of local institutions have developed techniques for the extraction and cleaning of fossil materials, derived from traditional methods in paleontology, especially in Kenya and South Africa. For the purposes of this paper, conservation efforts in paleoanthropology will be considered a separate literature and will not be covered.
Through the agency of international organizations several conservation scientists were able to travel widely sharing skills and initiating programs. One of these was Paul Coremans (1968:135–139; Tahk, 1984:16–25), whose energies and interests carried him from his base in Brussels at the Institut Royal du Patrimoine Artistique to sites in Indonesia, Burma, Thailand, Iran, Iraq, Peru, Mexico, and the United States of America.
F. Mairinger12 of the Insitut für Farbenlehre und Farbenchemie, Academie der Bildenden Künste, Vienna, recently visited China for the purpose of investigating analytical practice in conservation. He found their level of expertise based on pre-World War II technology, although they apparently are being influenced by Japanese experience and new Western methods.13
UNESCO, through its Museums and Monuments series, published a volume prepared by the International Centre for the study of the Preservation and Restoration of Cultural Property (Rome), now ICCROM, The Conservation of Cultural Property (1968). This was of special interest as it was written with reference to problems related to tropical conditions and situations with few technical resources. Articles were prepared by such workers as Daifuku from Bangkok and Andrade from Brazil. Other shorter documents have resulted from special seminars or conferences supported by UNESCO and ICOM. Among these are the reports written by Werner on the Conservation of Ethnographical Collections (1968) and Conservation of Cultural Materials in Humid Climates (Regional Seminar) published by the Australian National Conference for UNESCO in 1980.
In Argentina Tellchea (1981) produced a comprehensive text, Enciclopedia de la Conservacion y Restauracion, particularly designed for cultural materials found in South America and written for a wide audience, from craftsmen to conservators, as well as diverse environmental settings.
7 CONCLUSIONS
The development of conservation practice in archaeology and anthropology proceeded on a somewhat haphazard basis with European publications influencing American writers in a slow and uneven manner. The actual effect of these publications is questionable as treatments are scarcely mentioned in archaeological reports. In general, as Howie's results (1984) indicate for the field of paleontology and as seems consistent from the bibliographic material in this paper, methods and materials are easily introduced but resist rejection. Publication of new data on materials, rejection/repudiation of inferior techniques, and the introduction of new methods are slow to reach the majority of practitioners.
What this survey has shown is that there is a great need for conservators to offer courses in university anthropology departments and to offer reviews of general anthropology and archaeology texts, site reports and survey materials in order to expose archaeologists and anthropologists and their students to new trends in conservation. These reviews must be offered to journals in the field of anthropology and archaeology as well as appearing as presentations in national and regional conferences. A related problem is the lack of general texts in conservation and especially archaeological conservation.
Specialization in analytical and recovery techniques will most likely continue to benefit students of archaeometry rather than those minoring in conservation in university departments of anthropology. The largest number of university positions call for individuals who can still teach in several general survey and subject areas while pursuing specialized research, but we can hope that the trend of double masters (so frequently seen in England) of anthropologists with diplomas in conservation will increase.
The trend toward specialization in conservation is becoming an increasing reality in the graduation of conservation students from the various programs (NIC, 1984). This trend and the increasing number of retiring general practitioners in conservation will deny to the field the publication of generalized texts so prevalent in other fields and especially needed here to introduce archaeologists and their students to the field. The composition of such texts differs fundamentally from collections of articles written by different specialists, in that the experienced overview is drawn from years of study and experiment seasoned with examples of trial and error so necessary to learning. Such texts are the foundation of any discipline and, as the yearly swarm of introductory texts in every field proves, a necessary means of updating and focusing any body of organized knowledge.
The specter of so many experienced and older practitioners leaving the field by retirement without publishing summaries of their experience or outlines of their work in textbook form brings to the mind the plea of the 1923 Committee on Restoration and Preservation of Painting, Drawing and Prints (Museums J., 1923:118): “…it does seem necessary to issue a reminder that the absence of any official record of the measure of success or failure is an effectual barrier to the progress of knowledge upon the subject in question.” The publication of volume I of Herman Kühn's Conservation and Restoration of Works of Art and Antiquities by Butterworths (1986) is an exception which hopefully will become a trend.
NOTES
1. Brommelle (1956) describes a similar reaction to the early attempts at cleaning paintings in the National Gallery in England that led to the Select Committee Reports of 1850 and 1853.
2. Klaproth's paper was actually read publicly in 1795 but not published until two years later. Most authors, however, give Klaproth credit for the first publication even though a chemist named Pearson published a paper in 1796 and read in the same year (Caley, 1951:64; 1949:242).
3. Osgood's (1979) observations of storage conditions and conservation practice in American and Canadian museums present considerable evidence supporting this view. His recommendations for conservation treatments are out of date at best and are, at worst, examples of the need for scientific, standardized conservation practice.
4. N. L. Caldararo, unpublished report, “A Survey of University and College Course Offerings for Descriptions Containing References to the Conservation or Restoration of Artifacts or Specimens,” 1980.
5. Although the Bonnardot books among others (Brommelle, 1956; Ruhemann, 1968) were earlier, the presentations of Rathgen and Voss were the first systematic applications of scientific techniques (trans. note, Eng. ed. Rathgen, 1905). Rathgen's 1905 publication was most often quoted and referenced, though this two-volume “Handbücher” published between 1915 and 1924 is referenced by both Rowe (1953) and Heizer & Graham (1967).
6. Although certain segments of his paper have earned criticism for the “fragmented treatment” presented (Plenderleith, 1932: 508), many items were only described in outline.
7. This concept was argued by Pettenkofer (1870) with regard to paintings and was extended by Doerner (1934) to other art objects.
8. The National Conservation Advisory Council submitted a report, Proposal for a National Institute for the Conservation of Cultural Property (1982), which outlined a formal process and addressed the problems of the present situation; see pp. 26–27. Howie's recent research (1984) has shown the rapid application of new synthetic products and the slow rejection of materials found to be inappropriate for treatment. Another aspect of this is the reapplication of old techniques once rejected and reintroduced at a later date, such as in bleaching in paper conservation. A table such as Howie's could be constructed for bleaching showing the use of the hypochlorites; the use of hydrogen peroxide (Scott, 1926), its rejection (Hey, 1977) and reintroduction (Walsh, 1986); or the use of sugar in the stabilization of wood, its fall from favor and reintroduction (Parrent, 1985). Werner outlines the introduction of some synthetic materials in a 1968 report and later in a 1981 article.
9. Greathouse and Wessel's Deterioration of Materials (1954) provides data on the complexities of the process of deterioration of natural and synthetic materials, as well as descriptions of the disastrous results of material failing, when testing could not foresee the effects of varying climates and environments in combination with long-term oxidation, radiation and other factors.
10. Organ (personal communication, 1985) objects to this generalization which basically reflects published reports of work. As Organ points out, the demands of one's professional duties often forced practitioners to treat a wide variety of objects, yet a particular worker's publications may only reflect the most interesting challenges, a special interest, or only those specific treatments which he or she felt proposed the most significant contributions to the field. In the case of archaeology Organ's comments are even more appropriate: as the range of objects in most archaeological collections has demanded generalization in the practice of those who were charged with their care, as well as the composite nature of most archaeological and anthropological objects; this has been especially true of work on archaeological excavations.The situation has been changing, but specialization has had a much greater effect in other areas of the field of conservation, especially in paper and paintings. One particular example of the situation Organ mentions is that of George Stout, whose publications were generally in the area of Conservation of Fine Arts, mainly paintings, but whose influence and other unpublished contributions were considerable in other areas of conservation (Plenderleith, 1987). Also, his published works were often of such breadth that they could be applied to numerous problems and lines of inquiry in conservation as well as archaeology (e.g. the text on painting materials he published with Gettens in 1942).
11. E.g., B. C. Champion, “Identification et conservation des objets préhistoriqes,” Mouseion 16, (1931): pp. 35–47.
12. K.C. Chang (personal communication, 1982).
13. This view is consistent with that reported by T. Chase (1974), K.C. Chang (1977), and personal communication (1983); Colin Pearson in Museum, 32: 4: 1980, pp. 215–218; and Carol Snow (1985) and Haiwen (1985).
BIBLIOGRAPHY
Adamson, Helen. “Storage of Archaeological Material: the Problems.” The Museum Archaeologist3. (Society of Museum Archaeologists, April 1979).
Agrawal, O.P. “The Conservation Laboratory of the National Museum, New Delhi.” Studies in Conservation8, #5 (1963): pp. 99–105.
Agrawal, O.P., et al. Museum Techniques. Shahdara-Delhi, 1964.
Agrawal, O.P. “Conservation in South and South-East Asia.” Museum27, #3 (1975): 155–213.
Aitken, Martin. “Thermoluminescence and the Archaeologist.” AntiquityLI (1977): pp. 11–19.
Ambrose, Walter. “Conservation in the Field.” Kalori35 (Museum Association of Australia, 1968): pp. 34–45.
American Institute for Conservation. “Code of Ethics and Standards of Practice.” Annual Directory (Washington, D.C., 1980 et seg.).
Anonymous “Review of A. Lucas, Antiques: their Restoration and Preservation.” Museums Journal24 (1924): pp. 124–125.
Aoki, Shigeo. “Conservation of a Copper Statuette.” Science for Conservation24 (Tokyo, 1985): pp. 73–78.
Augusti, Selim. “Traitement de conservation de quelques objets de fouille en bois.” Studies in Conservation4, #4 (1959): p. 146–151.
Baer, N. S. “Chemical Aspects of the Conservation of Archaeological Materials.” American Chemical Society171 (1978) pp. 25–32.
Baer, N. S. & Majewski, L. J. “The History of Teaching in Conservation on the United States.” ICOM Committee for Conservation (4th Triennial Meeting, Venice, 1975): pp. 1–10.
Beck, Curt W. “Authentication and Conservation of Amber: Conflict of Interests.” Preprints, IIC Conference, Science and Technology in the Service of Conservation (Washington, D.C., 1982).
Bennett, H. G. “An Account of the Ancient Rolls of Papyrus, Discovered at Herculaneum, and the Method Employed to Unroll them.” Archaeologia15 (1806): pp. 114–117.
Biek, Leo. Archaeology and the Microscope. New York: Praeger, 1963.
Bonnardot, A.Essai sur l'Art de Restaurer les Estampes et les Livres. 1846. Reprint. New York: Burt Franklin, 1967.
Bourque, Bruce J., Brooke, Stephen W., Kelly, R., and Morris, K. “Conservation Archaeology: Moving toward Closer Cooperation.” American Antiquity45, #4 (1980): pp. 794–799.
Boustead, W. “The Conservation Department of the New South Wales Art Gallery, Australia.” Studies in Conservation (1960): pp. 121–131.
Boustead, W. “Conservation of Australian Aboriginal Bark Paintings.” Studies in Conservation2 (1966): pp. 197–204.
Brennen, Louis A.Beginner's Guide to Archaeology. New York: Dell, 1973.
Brommelle, Norman. “Material for a History of Conservation: the 1850–1853 Reports on the National Gallery.” Studies in Conservation2, #4 (October, 1956): 176–187.
Brothwell, Don A.Digging up Bones. London: British Museum, 1965.
Burns, Ned J.Field Manual for Museums. Washington, D.C.: National Park Service, 1941.
Butler, William. “The No-Collection Strategy in Archaeology.” American Antiquity44, #4 (October, 1979): pp. 795–799.
Byers, Douglas S. “The Restoration and Preservation of some Objects from Etowah.” American Antiquity28, #2 (1962): pp. 206–216.
Caldararo, Niccolo Leo. “Ethnographic Conservation: A Major Concern for Anthropologists.” Practicing Anthropology3, #2 (1980): pp. 39–40.
Caldararo, Niccolo Leo. “A Note on the Archaeological Report.” North American Archaeologist6, #1 (1984–5): pp. 63–80.
Caley, Earle R. “Klaproth as a Pioneer in the Chemical Investigation of Antiquities.” J. Chem. Education26 (May, 1949): pp. 242–248.
Caley, Earle R. “Early History and Literature of Archaeological Chemistry.” Journal of Chemical Education (February, 1951): pp. 64–66.
Chang, K.C. “Public Archaeology in China.” Paleo-Anthropology in the Peoples Republic of China. Edited by W. W.Howells & Patricia JonesTuchitari. CSCPRC Report #4 (National Academy of Sciences, 1977): pp. 130–139.
Chaptal, J.Report to the Academy of Sciences of Paris, 1787.
Chaptal, J. “Notice sur quelques couleurs trouvees a Pompeia.” Ann. Chim. 22 (1809): p. 70.
Chase, W. T. “Conservation in the Peoples Republic of China.” Bulletin, AIC 14, #2 (1974): pp.132–141.
Christensen, B.B.Om Konservering of Mosefudne Traegenstande. Copenhagen: National Museum, 1952.
Christenen, B.B. “Konservering af Moestrae Med Hjaelp af Tertiar Butylalkohol.” Aarboger for Nordisk Oldkyndighed og. Copenhagen: National Museum of Copenhagen, Historie, 1956.
Christenson, Andrew L. “Cultural Resource Management: The Role of Museums in Cultural Resource Management” American Antiquity44 (1980): pp. 161–163.
Clark, J. G. D.Excavations at Star Carr: An Early Mesolithic Site at Seamer near Scarborough, Yorkshire. Cambridge: University Press, 1954.
Clements, Forrest E. “Notes on Archaeological Methods: Excavation of Fragile Objects.” American Antiquity1, #3 (1936): pp. 193–207.
Conklin, Barbara. “New Storage at the American Museum of Natural History: Balancing Continuity and Change.” Curator23, #1 (1980): pp. 63–70.
Coremans, Paul. Problems of Conservation15. Paris: ICOM; Rome: ICCROM, 1969.
Craft, Meg and Jones, Sian. Written Documentation, AIC (9th Annual Meeting). Philadelphia: May 29, 1981. “The Curation of Archaeological Collections.” Curator23, #1 (Symposium Issue, 1980).
Davies, D. Gareth. “Museums and Archaeology—a Lost Cause?” Museums Journal (1978): pp. 123–125.
Davis, G. E.Chemical News36 (1877).
Davy, Sir H. “Some Observations and Experiments on the Papyri Found in the Ruins of Herculaneum” Phil. Translation of the Royal Society of London3 (1821): 191–208.
Davy, J. “Observations on the Changes which have Taken Place in some Ancient Alloys of Copper” Phil. Translation (1826): pp. 55, 116.
Directorate of Ancient Monuments and Historic Buildings, Department of the Environment. The Scientific Treatment of Material from Rescue Excavations: report by a working party of the Committee for Rescue Archaeology of the Ancient Monuments Board for England (1978).
Doerner, Max. The Materials of the Artist and their use in Painting with Notes on the Techniques of the Old Masters. 1921. Reprint in trans. New York: Harcourt, Brace and Co.
Dowman, Elizabeth. Conservation in Field Archaeology. Methuen & Co., 1970.
Faraday, Michael. “On the Ventilation of Lamp Burners.” London: Royal Institution Lecture, April 7, 1843.
Fielden, Bernard. “An Introduction to the Conservation of Cultural Property.” ICCROM, Rome. Paris: UNESCO.
Fielden, Bernard. personal communication, 1982.
Fink, Colin Garfield. “Incrustations on Porous Pottery: A New Method of Cleaning without Loss of Pigment.” Technical Studies in the Field of the Fine Arts2, #2 (October, 1933): pp. 58–61.
Fink, Colin Garfield. “Chemistry and Art.” Industrial and Engineering Chemistry26, #2 (February, 1934): pp. 234–238.
Florian, Mary-Lou E. “Fungicide Treatment of Eskimo Skin and Fur Artifacts.” Journal IIC-CG2, #1 (Autumn, 1976): pp. 10–17.
Florian, Mary-Lou E. and Dudley, David. “The inherent Fungicidal Features of Some Conservation Processes.” AIC Preprints (Dearborn, 1976): p. 41–47.
Florian, Mary-Lou E. “Waterlogged Artifacts: The Nature of the Materials.” CCI Journal2 (1977): 11–15.
Florian, Mary-Lou E. “Plant Material used in Some Ethnological Artifacts, Structure, Fabrication and Deterioration Related to Conservation Treatment.” AIC Preprints (Boston, 1977): pp.51–55.
Florian, Mary-Lou E., Seccombe-Hett, C. E., and McCawley, J. C. “The Physical, Chemical and Morphological Condition of Marine Archaeological Wood Should Dictate the Conservation Process.” Papers from the First Southern Hemisphere Conference on Maritime Archaeology (1978): pp. 128–144.
Florian, Mary-Lou E. “Analyses of Different States of Deterioration of Terrestrial Waterlogged Wood—Conservation Implication of the Analyses: A Review.” ICOM Com. for Conservation (6th Triennial Meeting, Ottawa, 1981).
Forbes, Robert James. Metallurgy in Antiquity—A Notebook for Archaeologists and Technologists. London: E. J. Brill, 1950.
Ford, Richard I.Systematic Research Collections in Anthropology: An Irreplaceable National Resource. Harvard University: Peabody Museum, 1977.
Ford, Richard I. “A Three-Part System for Storage of Archaeological Collections.” Curator23, #1 (March, 1980): pp. 55–62.
France—Lanord, A. “Le Polissage electrolytique et les repliques transparantes.” Studies in Conservation7, #4 (1962): pp. 121–134.
Frere, S., et al., a Working Party of the Committee for Rescue Archaeology of Ancient Monuments Board for England. The Scientific Treatment of Material from Rescue Excavations. London: Department of the Environment, 1978.
Fried, Stanley E. “Research Pitfalls as a Result of the Restoration of Museum Specimens.” The Research Potential of Anthropological Museum Collections, Annals of the New York Academy of Sciences (1981): pp.229–245.
Gairola, T. R.Handbook of Chemical Conservation of Museum Objects. University of Baroda: Dept. of Museology, 1960.
Gairola, T. R. “Setting up the Department of Preservation in the National Museum of India, New Delhi.” Curator3, #3 (1960): pp. 271–278.
Gallo, F.Patologia e Terapia del Libro. Rome: Raggio, 1951.
Garlake, Margaret. “Kitchen Conservation: Cleaning Corroded Iron.” South African Archaeological Bulletin22 (1967): p. 155.
Garlake, Margaret. “Cleaning Corroded Copper.” South African Archaeological Bulletin24 (1969): pp. 30.
Garlake, Margaret. “Recovery and Treatment of Fragile Artifacts from an Excavation.” South African Archaeological Bulletin24, (1969): pp. 61–62.
Gedye, I., and Hodges, H. W. “The Teaching of Archaeological Conservation.” Bulletin of the Institute of Archaeology, London University4 (1964): pp. 83–87.
Geidel, R. A. “Trace Element Studies for Mississippian Skeletal Remains: Findings from Neutron Activation Analysis.” Masca Journal2, #1 (June, 1982) 13–16.
Geijer, A., and Franzen, A. M. “Textile Conservation in Sweden: Problems and Practice.” Conservation in Archaeology and the Applied Arts, IIC (London: Stockholm Congress, 1975): pp.7–14.
Gettens, R. J. “Review of A. Lucas, Antiques: Their Restoration and Preservation” (2nd ed., revised, 1932). Technical Studies in the Field of Fine Arts2, #1 (July, 1933): pp.40–41.
Gettens, Rutherford J. and Stout, George L.Painting Materials. Van Nostrand Co., 1942; Dover Edition, 1966.
Gettens, Rutherford J. “The Corrosion Products of an Ancient Chinese Bronze.” J. Chem.Ed.28, #2 (1951): pp. 67–71. (From a 1950 Conference).
Gettens, Rutherford J. “Teaching and Research in Art Conservation.” Science133 (1961): pp. 1212–1216.
Gettens, Rutherford J. “IIC—An International Association of Conservation.” Museum News47, #10 (1969): pp. 11–14.
Gettens, Rutherford J.“Thoughts Apropos of a History of Conservation.” Unpublished manuscript presented at Cooperstown,N. Y. AIC meeting, 1974.
Goffer, Zui. Archaeological Chemistry: A Source Book on the Application of Chemistry to Archaeology. New York: John Wiley and Sons, 1980.
Graber, I. A.Problems of Restoration and Conservation of Objects of Art—a Methodical Guide. Moscow, U.S.S.R.: Academy of Arts, 1960; p. 190.
Greathouse, Glenn A. and Wessel, Carl J.Deterioration of Materials. New York: Reinhold, 1954.
Greene, Virginia. “Conservation of a Lyre from Ur.” Preprints of 7th Annual Meeting (AIC, 1979): pp. 37–43.
Grinsell, Leslie, Rahtz, P., and Warhurst, A.The Preparation of Archaeological Reports. New York: St. Martins Press, 1966.
Grosso, Gerald H. “After Excavation, then What?” Occasional Papers in Method and Theory in California Archaeology2 (Society for California Archaeology, 1978): pp. 53–58.
Guldbeck, Per E.The Care of Historical Collections. Nashville: American Association for State and Local History, 1972.
Haiwen, Wang. “The Care of Bronze Ware.” Palace Museum Journal2 (1985): pp. 74–78.
Heizer, Robert F.A Guide to Field Methods in Archaeology. Palo Alto: National Press, 1967.
Heizer, Robert F., and Graham, John A.A Guide to Field Methods in Archaeology, Palo Alto National Press, 1967.
HettCharles. “Archaeological Sites of the Canadian North: Their Preservation.” Journal of the Canadian Conservation Institute3 (1978): pp. 13–19.
Hey, Margaret. “Paper Bleaching: its Simple Chemistry and Working Procedures.” Paper Conservator2 (1977): pp. 10–23.
Higuchi, Seiji, and Aoki, Shigeo. “Conservation Treatment of Important Parts of Historic Sites by the Separation from the Mother Grounds.” Science for Conservation15 (1976): pp. 88–101.
Hitchcock, Ann. “Discussion Paper.” Curator23, #1 (March, 1977): pp. 71–79.
Hodges, H. W. M. “Problems and Ethics of the Restoration of Pottery.” Conservation in Archaeology and the Applied Arts (London: IIC, Stockholm Congress, 1975): pp. 37–38.
Hodges, H. W. M., and Hodkinson, I. S. “Training in Conservation: An Analysis.” ICOM Committee for Conservation (Venice: 4th Triennial Meeting, 1975): pp. 1–6.
Hole, Frank, and Heizer, Robert F.An Introduction to Prehistoric Archaeology. New York: Holt, Reinhart & Winston, 1965.
Holmes, William Henry, and Mason, Otis Tufton. “Instructions to Collectors of Historical and Anthropological Specimens.” U. S. National Museum Bulletin39, part Q (1902).
Howard, Marjorie M. “Field Treatment of Archaeological Specimens from Nimrud in Ivory.” Annual Report, University of London Institute of Archaeology11 (1953): pp. 71–74.
Howie, Francis M. P. “Materials Used for Conserving Fossil Specimens since 1930: A Review.” Adhesives and Consolidants (Preprints of the Paris Congress, IIC, 1984): pp. 92–97.
Huelsbeck, David R., and Wessen, Gary. “Thoughts on the Collection, Conservation, and Curation of Faunal Remains.” NARN16, #2 (1982): pp. 221–230.
Hulmer, E.The Role of Conservation on Connoisseurship. Ann Arbor, Mich.: University Microfilms, 1955.
Hume, Ivor Noel. Historical Archaeology. New York: Knopf, 1968.
Hurt, Wesley. “On the Preservation of Specimens and Museum Objects.” Museum Methods Lectures Delivered by Dr. Wesley Hurt at the University of California, Berkeley, 21–25 (Treganza Anthropology Museum, Spring, 1961).
International Museums Office. Manual on the Technique of Archaeological Excavations. Paris, 1940.
International Centre for the Study of the Preservation and Restoration of Cultural Property. The Conservation of Cultural Property. Rome: UNESCO, Museums and Monuments Series, 1968.
Irwin, Howard S., Payne, Willeard W., Bates, David M., and Humphrey, Philip S., eds.America's Systematic-Collections. Lawrence, KS: University of Kansas, 1973.
Ito, Nobuo. “Address.” International Symposium on the Conservation and Restoration of Cultural Property: Cultural Property and Analytical Chemistry (Tokyo National Institute of Cultural Properties, November 1978): pp. xi–xiii.
Janaway, Robert. “Textile Fibre Characteristics Preserved by metal Corrosion: The Potential of S. E. M. Studies.” The Conservator7 (1983): pp. 48–52.
Janoska, Peter. “The Conservation of Tin-Plated Bronze Objects from the Avar Period,” Marta, Jaro, ed.Problems of Completion, Ethics and Scientific and Scientific Investigation in Restoration (Budapest: 3rd International Restorer Seminar, Institute of Conservation and Methodology of Museums, 1982): pp. 96–100.
Jedrzejewska, Hanna. “Sampling Precautions in the Analysis of Metallic Antiquities.” Studies in Conservation7, #1 (1962): pp. 27–32.
Jedrzejewska, Hanna. “Some New Experiments in the Conservation of Ancient Bronzes.” Recent Advances in Conservation (London: Butterworths, 1963): pp. 135–139.
Jedrzejewska, Hanna. “The Conservation of Ancient Bronzes.” Studies in Conservation9, #1 (1964).
Jedrzejewska, Hanna. “A Corroded Egyptian Bronze: Cleaning and Discoveries.” Studies in Conservation21, #3 (1976): pp. 101–114.
Johnson, Ernst N. “Preservation and Cleaning of Shell Material.” SSA Notebook2, #1 (April, 1941): pp. 9–12.
Joukousky, Martha. A Complete Manual of Field Archaeology. Englewood Cliffs, NJ: Prentice-Hall, 1980.
Kabaivanov, V., and Mitanov, P. “Attempts at Stabilizing Art Works Made of Wood or with a Wooden Support by Permeation with Monomers and Monomer Mixtures and the Resulting Polymerization.” Museums and MonumentsXIV, #4 (1974): pp. 46–58.
Keel, Bennie Carlton. “The Conservation and Preservation of Archaeological and Ethnological Specimens.” Southern Indian Studies15 (October, 1963): pp. 5–65.
Kennedy, Robert A. “Conservation in the Wet Tropics.” Technical Bulletin of the Museums Association of Middle Africa1 (1959): p. 12.
King, Mary Elizabeth. “A Comment and Warning.” Anthropology in Museums of Canada and the U. S.Cornelius Osgood as reviewed by James Deets, Council for Museum Anthropology Newsletter6, #3 (1982): pp. 25–26.
King, Mary Elizabeth. “Curators: Ethics and Obligations.” Curator23, #1 (March, 1980): pp. 10–18.
Klaproth, Martin Heinrich. “Memoire de Numismatique Docimastique.” Memoires de l'Academie Royal des Sciences et Belles Lettres (Berlin: Classe de Philosophie Experimentale, 1798): pp. 97–113.
Korostovetz, A. R. A., and Thomson, G. “Review of Problems of Restoration and Conservation of Objects of Art.” Studies in Conservation8, #2 (Moscow, May, 1963): pp. 73–76.
Kühn, Hermann. Conservation and Restoration of Works of Art and Antiquities, 1. London: Butterworths, 1986.
Laudermilk, J. D. “The Preservation of Textile Remains.” American Antiquity4 (1937): pp. 277–281.
Lee, Mary Wood. Personal communication, 1978.
Lee, Welton L., Bell, Bruce M., and Sutton, John F.Guidelines for Acquisition and Management of Biological Specimens. Lawrence, KA: Association of Systematic Collections, Museum of Natural History, University of Kansas, 1982.
Leechman, Douglas. “Technical Methods in the Preservation of Anthropological Museum Specimens.” Annual Report, 1929 (National Museums of Canada, Bulletin67, 1931): pp. 127–158.
Leigh, David. First Aid for Finds 1. University of Southhampton: Rescue and the Department of Archaeology, 1978.
Leigh, David. “The Selection, Conservation and Storage of Archaeological Finds.” Museums Journal2 (September, 1982): pp. 115–116.
Lerici, Carlo Maurilio. “Methods used in the Archaeological Prospecting of Etruscan Tombs.” Studies in Conservation6, #1 (1961): pp. 1–8.
Lewis, Ralph H.Manual for Museums. Washington, D. C.: National Park Service, 1976.
Lightbody, Albert, Roberts, Merritt E., and Wessel, Carl. “Plastics and Rubber.” Deterioration of Materials. Greathouse, Glenn A., and Wessel, Carl, eds.New York: Reinhold, 1954.
Lindsay, A.J., Jr.The Curation and Management of Archaeological Collections: A Pilot Study. Washington, D. C.: American Anthropological Association, 1979.
Lindsay, A,J., Jr., and Williams Dean, Glenna. “Artifacts, Documents, and Date: A New Frontier for American Archaeology.” Curator23 (1980): pp. 12–29.
Lloyd, Allan. “One Hundred Years of Art Restoration/Conservation at the Art Gallery of New South Wales.” ICCM Bulletin7, #2/3 (September–December, 1981): pp. 3–15.
Loy, Thomas H. “Prehistoric Blood Residues: Detection on Tool Surfaces and Identification of Species of Origin.” Science220 (June 17, 1983): pp. 1269–1271.
Loy, Thomas H. “Archaeological Collections and the Trash Bin Syndrome.” NARN16 (Fall, 1982): pp. 201–205.
Lucas, A.Antiques: Their Restoration and Preservation. London: Edward Arnold, 1924; 2nd ed., 1932.
MacDonald, George F. “The Problems and Promise of Wet Site Archaeology.” Journal of the Canadian Conservation Institute2, (1977): pp. 3–10.
Macintosh, N.W.G. “The Recovery and Treatment of Bone.” Australian Archaeology: A Guide to Field Techniques. Canberra: Institute of Aboriginal Studies, 1968.
Marquardt, William H., ed.Regional Centers in Archaeology: Prospects and Problems14. Columbia, Missouri: The Missouri Archaeological Society, 1977.
Mauger, Jeffery E. “Archaeological Preservation and the Future of Archaeology.” NARN16, #2 (Fall, 1982): pp. 188–192.
McCarthy, F.D.Aboriginal Antiquities in Australia: Their Nature and Preservation. Australian Aboriginal Studies, 22; Prehistory and Material Cultural Series, 3. Canberra, 1970.
McCawley, J.C. “Waterlogged Artifacts: The Challenge to Conservation.” CCI Journal2 (1977): pp. 16–21.
McGrimsey, Charles R.III, and Davis, Hester A.The Management of Archaeological Resources: The Arlie House Report. Washington, D.C.: Society for American Archaeology, Special Publication, 1977.
Meurgues, Genevieve. “Errors of Treatment: Synthetic Resins can be Dangerous.” Museum34, #1 (1982): pp. 60–61.
Morgan, R.A., Hillan, J., Coles, J.M. and McGrail, S. “Reconciling Tree-Ring Sampling with Conservation.” Antiquity55, #214 (July, 1981).
Morris, Kenneth, and Seifer, Betty I.. “Conservation of Leather and Textiles from the Defense.” JAIC18, #1 (Autumn, 1978): pp. 43–45.
Mühlethaler, Bruno. Conservation of Waterlogged Wood and Wet Leather. Paris: International Centre for the Study of Preservation and Restoration of Cultural Property 11, 1973.
Mühlethaler, Bruno. Kleines Handbuch der Konservierungstechnik (A Concise Handbook of Conservation Technique). Bern and Stuttgart: Verlag Paul Haupt, 1967.
National Institute for the Conservation of Cultural Property. The History and Future Directions of Conservation Training in North America. Washington, D.C., 1984.
Neustupny, Jiri. Museum and Research. Office of Regional and Museum Work of the National Museum in Prague, 1968.
Nogid, I., and Rozdnyak, A. “Conservation of Waterlogged Wood.” Soviet Archaeology3 (Moscow, 1965): pp. 277–279.
Novick, Andrea Lee. “The Management of Archaeological Collections.” Curator23, #1 (1980): pp. 30–42.
Oddy, W.A., Hughes, M.J. “The Stabilization of ‘Active’ Bronze and Iron Antiquities by the Use of Sodium Sesqui-Carbonate.” Studies in Conservation15, #3 (1970): pp. 183–189.
Oddy, W.A., “Review of Elizabeth Dowman, Conservation in Field Archaeology.” Studies in Conservation18, #1 (February, 1973): pp. 44–45.
Oddy, W.A. “The Corrosion of Metals on Display.” Conservation in Archaeology and the Applied Arts (London: IIC Stockholm Congress, 1975): pp.235–237.
Oddy, W.A. “The Conservation of Pyritic Stone Antiquities.” Studies in Conservation22, #2 (1977): pp. 68–72.
Organ, R.M. “Reclamation of Silver from the Wholly Mineralized Ur Lyre.” The Application of Science to Examination of Works of Art (Museum of Fine Arts, Boston, 1967): pp. 126–144.
Organ, R.M.Design for Scientific Conservation of Antiquities. Washington, D.C.: Smithsonian Institution Press, 1968.
Organ, R.M. “Information Required in a Published Report of Analysis in Order that the Report Shall Possess Value as Evidence for Museum Purposes.” ICOM Conservation Committee, #29, September, 1969: p. 8930.
Organ, R.M. “Problems of the Museum Laboratory.” Proc. Second ISCRSP, Cultural Property and Analytical Chemistry (Tokyo, 1979): pp. 24–27.
Osgood, Cornelius. Anthropology in Museums of Canada and the U.S.7. Milwaukee Press, 1979: pp. 80–83.
Otto, Helmut. “Das Chemische Laboratorium der Königlichen Museum in Berlin.” Berliner Beitrage Zur Archäometrie4 (1979).
Packard, Elizabeth C.G. “Conservation Goes Public: George Stout and the Art Technical Sections (AAM).” AIC Preprints (1979): pp. 86–93.
Packard, Elizabeth C.G. “George Stout and the Art Technical Sections of the AAM Annual Meetings in the 1930s and 1940s, Part II.” AIC Preprints (1980): pp. 72–83.
Parrent, James M. “The Conservation of Waterlogged Wood Using Sucrose.” Studies in Conservation30 (1985): pp. 63–72.
Pappas, Peter S., and Winslow, F.H.Photodegradation and Photostabilization of Coatings151. Washington, D.C.: American Chemical Society Symposium Series, 1981.
Patoharju, Ora. “Conservation of Cannon Recovered from the Brackish Sea.” Conservation in Archaeology and the Applied Arts. London: IIC Stockholm, 1975.
Pelikan, J.B. “The Use of Polyphosphate Complexes in the Conservation of Iron and Steel Objects.” Studies in Conservation9 (1964): pp. 59–66.
Pelikan, J.B. “Conservation of Iron with Tannin.” Studies in Conservation11, #3 (1966): pp. 109–115.
Peterson, Curtis. “The Nature of Data from Underwater Archaeological Sites.” Underwater Archaeology—The National Park Service (DanielLenihan, ed., Division of Archaeology S.W. Region, National Park Service, July, 1974): pp. 62–65.
Pettenkofer, Maxvon. Uber Ölfarbe und Konservierung der GeraldeGallerien durch das Regeneration-Verfahren. Braunschweig, Friedr. Vieweg, 1870.
Plenderleith, H.J. “Review of Technical Methods…by D. Leechman.” Museums J.31 (1932): p. 507.
Plenderleith, H.J.Preservation of Antiquities. London, 1934.
Plenderleith, H.J.The Conservation of Prints, Drawings and Manuscripts. London: The Museums Association, Oxford University Press, 1937.
Plenderleith, H.J. “The Conservation of Archaeological Groups and of the Objects Discovered.” Manual on the Technique of Archaeological Excavations (IMO, Paris, 1940).
Plenderleith, H.J.The Conservation of Antiquities and Works of Art. London: Oxford University Press, 1956.
Plenderleith, H.J., and Torraca, G. “The Conservation of Metals in the Tropics.” The Conservation of Cultural Property. Rome: UNESCO ICSPRCP, 1968.
Plenderleith, H.J., and Werner, A.E.A.The Conservation of Antiquities and Works of Art, 2nd. ed.London: Oxford University Press, 1971.
Plenderleith, H.J.Personal communication, 1987.
Rathgen, Friedrich. The Preservation of Antiquities. Cambridge: The University Press, 1924.
Rathgen, Friedrich. Die Konservierung von Altertumsfunden, mit Berücksichtigung Ethnographischer und Kunstgewerblicher Sammlungsgegenstände, Handbücher der Königlichen Museen zu Berlin VI. Berlin and Leipzig: 1915–1924.
Reed, R.Ancient Skins, Parchments and LeathersLondon: Seminar Press, 1972.
Rhoussopoulos, D.A. “On the Cleaning and Preservation of Antiquities.” Museums Journal (November, 1911): pp. 131–144.
Riederer, Josef. “The Rathgen Research Laboratory at Berlin.” Studies in Conservation21, #2 (1976): pp. 67–73.
Robbins, Maurice. The Amateur Archaeologist's Handbook. New York: Thomas Y. Crowell, 1965.
Rose, Carolyn. “Notes on Archaeological Conservation.” AIC Bulletin, 14, #2 (1974): pp. 128–130.
Rose, Carolyn. “An Introduction to Museum Conservation.” American Indian Art Magazine3, #1 (November 1, 1977).
Rosenberg, Gustave Adolf Theodor. “Antiquities en fer et en bronze, leur transformation dans la terre contenant de l'acide carbonique et des chlorures et leur conservation.” Ouvrage Publié par la Fondation Carlsberg. Gyldendalske Boghandels Sortiment, Kobenhavn, 1917.
Rosenberg, Gustave Adolf Theodor. “The Preservation of Antiquities of Organic Material.” Museums J.33 (March, 1934): pp. 432–436.
Rosenqvist, Anna M. “The Stabilizing of Wood Found in the Viking Ship of Oseberg,” part 1. Studies in Conservation4, #1 (1959): pp. 13–22.
Rosenqvist, Anna M. “The Stabilizing of Wood Found in the Viking Ship of Oseberg,” part 2. Studies in Conservation4, #2 (1959): pp. 62–72.
Rowe, J.H. “Technical Aids In Anthropology: An Historical Survey.” Kroeber, A.L., ed.Anthropology Today. Chicago: University of Chicago Press, 1953.
Ruggles, M. “The History of Conservation in Canada: Developments to the early 1970s.” Journal of the IIC-CG5, #1/2 (Spring, 1980): pp. 3–12.
Ruhemann, Helmut. “The Cleaning of Paintings.” New York: Praeger, 1968.
Sanna Ullah, Mohammad. “La Conservation des objets en cuivre déteriorés par une ambiance saline.” Mouseion25–26 (1934).
Santucci, S. “Application of Chemical Methods to the Treatment of Works of Art.” Recent Advances in Conservation. London: Butterworths, 1963.
Saunders, C. “Archaeology and Museums—Another View.” The Museum Anthropologist (London, Society for Museum Anthropologists, 1979): pp. 10–19.
Schaffer, E. “Consolidation of Softwood Artifacts.” Studies in Conservation16 (1971): pp. 110–113.
Schaffer, E. “Properties and Preservation of Ethnological Semi-tanned Leather.” Studies in Conservation19 (1974): pp. 66–75.
Schaffer, E. “The Preservation and Restoration of Canadian Ethnographic Basketry.” Studies in Conservation21 (1976): pp. 129–133.
Schaffer, E. “Fiber Identification in Ethnographical Textile Artifacts.” Studies in Conservation26 (1981): pp. 119–129.
Schenk, Robert. “Museology, the Laboratory Sciences.” Handbook. San Francisco: Department of Anthropology, San Francisco University, 1967.
Schur, Susan E. “Laboratory Profile: The Conservation Services Laboratory of the Detroit Institute of Arts.” Technology and Conservation8, #3 (Fall, 1983): pp. 26–40.
Schur, Susan E. “Laboratory Profile: The Anthropology Conservation Laboratory, Smithsonian Institution.” Technology and Conservation6, #4 (Winter): pp. 26–35.
Scott, Alexander. “The Cleaning and Restoration of Museum Exhibits” (report upon investigation conducted at the British Museum, Department of Scientific and Industrial Research). Bulletin5 (London: His Majesty's Stationery Office, 1921): pp. 1–13.
Scott, Alexander. “The Cleaning and Restoration of Museum Exhibits.” 2nd Report. British Museum, Dept. of Scientific and Industrial Research. (London: H.M. Stationery Office, 1923): pp. iii–11.
Scott, Alexander. “The Cleaning and Restoration of Museum Exhibits.” 3rd Report. British Museum, Dept. of Scientific and Industrial Research. (London: H.M. Stationery Office, 1926): pp. iii–70.
Sease, Catherine. “The Case Against Using Soluble Nylon in Conservation Work.” Studies in Conservation26, #3 (1981): pp. 102–110.
Singley, Katherine R. “Caring for Artifacts after Excavation—Some Advice for Archaeologists.” Historical Archaeology15, #1 (1981): pp. 36–48.
Snow, Carol E. “Conservation of Cultural Relics in the People's Republic of China.” AIC Preprints (Washington, 1985): pp. 101–112.
South, Stanley. “The Role of the Archaeologist in the Conservation Process.” Preservation and Conservation: Principles and Practices. Timmons, S., ed.National Trust for Historic Preservation: The Preservation Press, 1976.
Stambolov, T.Manufacture, Deterioration and Preservation of Leather: A Literature Survey of Theoretical Aspects and Ancient Techniques. Amsterdam: ICOM, 1969.
Stanley-Price, N., ed.Conservation on Archaeological Excavations, with Particular References to the Mediterranean Area. Rome: ICCROM, 1984.
Stansfield, G. “The Storage of Museum Collections.” Museum Association Information Sheet10 (revised, Museum Association, 1977): pp. 1–5.
Stoner, Joyce Hill. “An Oral History Archive: Conservation.” Museum News (July/August, 1977): pp. 9–12.
Stucker, Gilbert F. “Review of A.E. Rixon, Fossil Animal Remains: Their Preparation and Conservation.” Studies in Conservation22, #4 (1977): pp. 200–201.
Swarnakamal. Protection and Conservation of Museum Collection(s). Baroda: Museum and Picture Gallery, 1975.
Tahk, F. Christopher. “A Brief History of the Art Conservation Department of the State University of New York College at Buffalo.” The History and Future Direction of Conservation Training in North America (National Institute for the Conservation of Cultural Property, December, 1984): pp. 16–25.
Tellechea, Domingo I.Enciclopedia de la Conservation y Restauracion. Argentina: Editorial Techno-transfer S.R.L., 1981.
Thompson, Jack. “Conservation in New Zealand.” WAAC Newsletter7, #3 (1985): pp. 13–14.
Thomson, Garry. The Museum Environment. London: Butterworths, 1978.
Tomashevich, G.N. “The Conservation of Waterlogged Wood.” Problems of Conservation in Museums8 (ICOM, Allen & Unwin, 1969): pp. 165–186.
Todd, William. “A Vacuum Process for the Preservation of Bone and Similar Materials.” Technical Studies in the Field of the Fine Arts9, #3 (January, 1941): pp. 160–164.
Todd, William. “Iron Armatures and Supports in Chinese Grave Figurines.” Royal Ontario Museum of Archaeology Bulletin18 (March, 1952): pp. 17–18.
Torraca, G.Solubility and Solvents. Rome: ICCROM, 1975.
UNESCO. Conservation of Cultural Materials in Humid Climates. Canberra: Regional Seminar, Australian National Committee for UNESCO, 1980.
VanGalik. Chinese Pictorial Art as Viewed by the Connoisseur. Rome: Inst. Itale per il Medio Ed. Est. Orh., 1958.
Velich, Ralph. “The Repair and Cleaning of an Old Painted Buffalo Robe.” Curator8, #4 (1965): pp. 319–324.
Voss, A. “The Excavation and Preservation of Antiquities.” MerkbuchBerlin: 2nd ed., 1894.
Walsh, Judith C. “Special Conservation Problems for Collectors—the Cleaning of Drawings.” Drawing8, #1 (May/June, 1986): pp. 4–7.
Ward, Phillip. “The State of Preservation of the Native Heritage on the Northwest Coast”. Journal of the Canadian Conservation Institute3 (1978): pp. 4–9.
Waterer, John W.A Guide to the Conservation and Restoration of Objects made Wholly or in Part of Leather. London: Camelot Press, 1972.
Weill, A.R. “Etude et nettoyage non-destructifs d'une piece d'orfevrerie morovingienne provenant de Saint-Denis, Seine.” Studies in Conservation4, #4 (1958): pp. 121–126.
Werner, A.E.A., and Thompson, G.Synthetic Materials Used in the Conservation of Cultural Property. Rome: ICSPRCP Works and Publications, v. 5, 1963.
Werner, A.E.A., “The Conservation of Ethnographical Collections.” Report presented to the ICOM Committee on Conservation, Amsterdam, Sept. 13–19, 1969.
Werner, A.E.A. “Synthetic Materials in Art Conservation”. Journal of Chemical Education58, #4 (April, 1981).
Wheeler, Sir Mortimer. Archaeology from the Earth. Oxford: 1954.
White, J. Peter. “Report Writing and Publication.” Australian Field Archaeology: A Guide to Techniques (Canberra, Australian Institute of Aboriginal Studies, 1983): pp. 171–178.
Wilcox, U. Vincent. “Collections Management with the Computer.” Curator23, #1 (1980): pp. 43–52.
Winkelman, Johann Joachim. A Critical Account of the Situation and Destruction of Herculaneum and Pompeii. T.Carnan and F.Newberry, 1771.
Wolf, Sara J. and Mibach, Lisa “Ethical Considerations in the Conservation of Native American Sacred Objects.” Journal of the AIC23, #1 (Fall, 1983): pp. 1–6.
Woodward, C.J. “The Action of Gas on Leather Bookbindings: A Preliminary Experimental Inquiry.” The Library Chronicle5 (1888): pp. 25–29.
Woolley, Sir Charles Leonard. Ur Excavations II: The Royal Cemetery. London: 1934.
Yamasaki, Kazuo. “Review of Conservation of Old Art Objects.” Studies in Conservation3, #2 (October, 1957): pp. 83–88.
Section Index |