JAIC 1991, Volume 30, Number 1, Article 2 (pp. 03 to 11)
JAIC online
Journal of the American Institute for Conservation
JAIC 1991, Volume 30, Number 1, Article 2 (pp. 03 to 11)

CONSERVATION TREATMENT OF TIBETAN THANGKAS

ANN SHAFTEL



3 SPECIFIC EXAMPLES OF INAPPROPRIATE TREATMENTS

THE FOLLOWING examples are drawn from thangkas owned by The Nelson-Atkins Museum of Art, Kansas City, Missouri. The author has extensively researched these thangkas, completed conservation study, and begun conservation treatment. It should be noted that the thangkas used here as examples had been treated before they entered the collection of the museum; The Nelson-Atkins Museum of Art is to be respected for the care of its collection.


3.1 EXAMPLE 1

Gelukpa Assembly Field, 74-36/18, Nelson-Atkins Museum of Art (Bequest of Joseph H. Heil) h. 76.2 × w. 117.5 cm; overall dimensions: h. 154 × w. 169 cm (fig. 2)

Fig. 2a. Gelukpa Assembly Field, Tibetan, 19th century, Nelson-Atkins Museum of Art, Kansas City, Missouri (Bequest of Joseph H. Heil) 74-36/18. Detail, proper lower right corner of painting. The painting support was not relaxed before lining as the lining was carried out with the painting in place in its mounting.

Fig. 2b. Detail proper lower right corner, reverse. The Mylar is split and is peeling away from the polyvinyl acetate. Pools of bubbled polyvinyl acetate. Pools of bubbled polyvinyl acetate fill irregularities in the support from behind, reinforcing the uncomfortable fit of the support in its mounting.

This is an example of conservation treatment in situ in its mounting. The following is a brief summary of the condition; it is not intended as a complete examination report.

The mounting of this thangka is traditional and elaborate. The cover is in comparatively good condition. According to a museum employee, it was folded behind the mounting while the thangka was on exhibit continuously for 10 years. The cover is of hand-stitched silk with two panels crowned by an elaborate valence. The mounting proper has leather corners, hanging ribbons, and other traditional components. Both original dowels are missing; the bottom edge of the mounting has been trimmed off, then crudely sewn to create a new dowel sleeve.

The painting support is of medium-weight plain-weave cotton. It is damaged overall with the creases and folds common to older thangka painting supports. The ground and paint layers reflect the damage to the support below. The ground was originally off-white in color and finely applied and polished. The paint layers were originally skilfully applied but are now faded, dirty, and abraded with a network of losses overall.

The support has been lined on the reverse with polyvinyl acetate (PVA-AYAA) onto thin Mylar, carried out with the painting in place in its mounting. For several reasons, it cannot be considered a successful endeavor.

First, the support was not flattened before lining. The creases, wrinkles, and bulges were not allowed to relax into a planar surface before the lining process. Pools of bubbled polyvinyl acetate fill irregularities in the support from behind. The polyvinyl acetate has a top surface contour similar to a landscape—with mountains, valleys, and plains. Any draws or buckles caused by the uncomfortable fit of the cotton support of the painting into the silk mounting have been reinforced.

On the reverse the thin-gauge-Mylar is peeling away from the polyvinyl acetate in the proper lower right-hand corner. On the obverse, specular reflection shows glints of shiny adhesive that has come up through areas of weakness in the support. No attempt has been made to remove these, nor has any inpainting been attempted.

In summary, the painting was lined in situ. The painting was not made planar prior to lining, so surface irregularities were reinforced. The Mylar lining is peeling off, and the adhesive has leaked through the support and glistens on the obverse. No treatment has been given to the mounting.

This thangka has received a treatment inadequate for its preservation. Reversal and correction of the above treatment would be difficult and require extensive use of solvents.


3.2 EXAMPLE 2

The Dharmapala Paldan Lhamo (Glorious Goddess) and Her Retinue 74-36/26, Nelson-Atkins Museum of Art (Bequest of Joseph H. Heil), h. 80 × w. 57.1 cm; overall dimensions: h. 80.6 × w. 58.8 cm (fig. 3)

Fig. 3. The Dharmapala Paldan Lhamo (“Glorious” Goddess) and Her Retinue, Tibetan, 18th century, Nelson-Atkins Museum of Art, Kansas City, Missouri (Bequest of Joseph H. Heil) 74-36/26. Front, overall, painting only, no mounting remaining. The surface is flat and dead.

This is an example of a painting permanently separated from its mounting and lined with a “heavy hand.” The following is a brief summary of the condition.

The support is medium-weight plain-weave cotton. Raking light shows a planar surface except for a 7.1 cm long crease located in the proper lower right quadrant and running diagonally. Transmitted light shows areas of former weakness in the support of a type often found in thangkas that have been rolled and handled improperly. The ground is off-white and evenly applied on both sides of the support. The background color of the composition is black, the traditional color for a painting that depicts a protector of the teachings.

The ground and paint layers are secure, but the colors have a flat, dead surface from the lining process and are darkened from adhesive penetration. These colors can be contrasted to the other original colors still visible on the untreated tacking edge, which have varied textures and are lighter, and more “alive.”

On the obverse, the conservator neglected to remove each thread (which originally held the painting in its mounting) before beginning the lining process. Consequently, fragments of cotton threads still remain in some of the stitch holes in the tacking edge.

On the reverse, these thread fragments are partially embedded in the mounting adhesive and partially covered by the Mylar lining. This lining does not completely cover the reverse of the support but extends unevenly up to the tacking edge.

This painting has been given a conservation treatment that, even if applied to a Western painting, would be inappropriate considering the results achieved. It was lined with polyvinyl acetate (PVA-AYAA) on Mylar with a brush coat of the liquid adhesive in toluene. Some of the adhesive penetrated through the ground and paint layers to the front of the painting. Then it was lined face up on a vacuum hot table with a high vacuum (24″ Hg), which created weave interference by forcing the paint film down into the weave of the support fabric. This treatment irreversibly altered the painting both physically and aesthetically.

The flat quality the painting now has destroys the effect of varied textures of each type of pigment. Traditionally, some of the colors (blues and greens) would have been burnished after being applied and others, such as the traditional red, would have had a shiny surface. The flat gold and the shiny gold details in the flames and on the garments would catch the light in yet a different way. When this surface was viewed in the candlelight and butterlamp light of shrines, the surface would appear rich in texture, with flashing and glittering gold highlights. In this case, inappropriate conservation treatment has obliterated these effects. The surface has a dead, dull quality instead of a lively aspect that would express the life and power of the deities depicted.


3.3 EXAMPLE 3

An Enthroned Buddha, 35-134/1, Nelson-Atkins Museum of Art (Nelson Fund), h. 123 × w. 73 cm; overall dimensions: h. 142 × w. 84 cm (fig. 4)

Fig. 4. An Enthroned Buddha, Chinese Lamaistic, 19th century, Nelson-Atkins Museum of Art, Kansas City, Missouri (Nelson Fund) 35-134/1. The painting has been removed from the orginal mounting and remounted in Chinese scroll form. It is no longer a complete thangka.

This is an example of a painting removed from a thangka and remounted in China.

The current mounting is thin silk on paper, Chinese style. The mounting is shredded on the outside edges of the top section. A small section of the mounting silk is missing from the proper left side panel (at the level of the Buddha's head). The proper upper left corner bears a stain. The mounting is not in traditional Tibetan style in form, color, or proportion.

The painting support is a traditionally prepared plain-weave cotton cloth. From the pattern of visible damage to the ground and paint layers, one can assume that the support was creased and cockled prior to lining. Currently, the support is relatively stable with a repetitive series of bulges corresponding to the pattern as rolled. The ground and paint layers were applied in traditional manner and are currently stable but show evidence of previous damage. There is overall paint loss corresponding to former creases in the support. A second category of paint loss appears to be the result of abrasion. A third category is water damage, with total loss of paint layers in some areas.

The fourth category of damage to the ground and paint layers is the direct result of the Chinese mounting process, which introduces moisture from behind and employs an aqueous adhesive. Both techniques cause the delicately applied paint layers to sink into each other. A matte and slightly blanched surface is the result.

This surface is not in keeping with the original intent of the artist. In traditional Himalayan thangka painting the desired effect of a finished painting is a marked texture variation across the surface. Flat contrasts with burnished areas, thin washes contrast with more heavily applied pigments, dry shading contrasts with wet. The various sizes of particles of traditional pigments create a varied surface texture. The organic lakes used for shadow and outline are thin and fine, without a granular texture at all. The aesthetic is almost three-dimensional in its effect, not at all the flat matte, sunken surface created by a Chinese or Japanese mounting process.

A thangka is not only a painting; hung properly, it creates a three-dimensional sculpture. The raised and draped cover, the ribbons hanging partially over the painting, and the finials of the bottom dowel curving out from the mounting all contribute to this effect. Even a recently made painting in its mounting does not present a perfectly planar surface, in contrast with the flat painting and mounting surfaces of Chinese and Japanese scroll paintings.

Paintings similar in content to Tibetan thangkas have been created in China with Chinese aesthetics. Mountings are flat, in scroll form with paper backing. But a Tibetan creation does not take kindly the removal from its original cloth mounting and the flattening in Chinese scroll form. A thangka is not only the painting but the mounting and the painting combined. The iconography suffers from the change. The top, bottom, and side panels bear a size relationship set by tradition and by regional style and subject matter. A foreign, albeit geographically close, aesthetic cannot but diminish the traditional creation.


Copyright © 1991 American Institute for Conservation of Historic and Artistic Works