THE HISTORY AND SIGNIFICANCE OF THE SCHREGER PATTERN IN PROBOSCIDEAN IVORY CHARACTERIZATION
EDGARD O'NIEL ESPINOZA, & MARY-JACQUE MANN
5 OBSERVATIONS AND DISCUSSION
We obtained intertusk Schreger angle data from the outside pattern area to document angle variance within and along a single tusk. Five convex and five concave outside angle measurements were obtained from each of 16 sequential sections taken from a Loxodonta africana tusk approximately 90 cm x 12.5 cm.
Pooled convex angle and concave angle measurements from tusk sections ranged between 134.5° and 143° (average = 139.1°, standard deviation = 2.37) with no significant variance observed from section to section. Sectional convex and concave angle data were then converted to radians for statistical purposes and compared to each other by t-test statistic with p<0.05 considered significant. The t-test statistic tests the hypothesis (HO) that there is no difference between the convex and concave angle data, where p<0.05 represents the smallest value that would lead to rejection of the hypothesis. No significant difference was observed between the convex and concave Schreger angles within the outside area of a tusk.
Five convex and five concave outside Schreger angle measurements were taken from each Loxodonta and Elephas (n = 26), and from each Mammuthus primigenius (n = 26) tusk sample. For elephant the combined average was 124.2° (standard deviation = 9.28) with a range from 95° to 163°; for mammoth the average was 73.7° (standard deviation = 9.76) with a range from 35° to 115°. Radian-transformed convex and concave angle data from each tusk sample were compared by t-test statistic, with p<0.05 considered significant. No significant statistical difference was observed between convex and concave Schreger angles within individual samples. Since no differences were observed, the data from each tusk sample were averaged to get a single value to represent each individual.
Radian-transformed mean data from each of the 26 elephants and 26 mammoth samples were compared by t-test statistic with p<0.05 considered significant. The t-test statistic tests the hypothesis (HO) that there is no difference between the angle data from extinct and modern samples, where p<0.05 represents the smallest value (t.95 = ± 1.671) that would reject the hypothesis. The statistical analysis rejected the hypothesis and showed that the differences in Schreger angle means in modern versus extinct proboscidean samples are statistically significant (t = 19.42). Table 1 shows the distribution in degrees and radians of the mammoth and elephant sample data. Figure 2 presents a graphic summary of all the outer Schreger Pattern angles of extinct and modern proboscidean ivory samples measured for this study. Although not included in the data set, the Schreger angles of three Gomphotherium and three mastodon tusk samples fell within the range (35°–115°) observed in mammoth samples.
TABLE 1 DISTRIBUTION IN RADIANS AND DEGREES OF MAMMUTHUS PRIMIGENIUS AND LOXODONTA/ELEPHAS SCHREGER PATTERN ANGLE MEANS
Fig. 2.
Histogram of all outer Schreger Pattern angles of extinct and extant Proboscidean ivory samples (N = 260 each). This figure is reprinted from Identification guide for ivory and ivory substitutes with permission from the World Wildlife Fund.
 |
Schreger Pattern outer angles in proboscidean ivories clearly differentiate between extinct (legal) and modern (illegal) sources, and micromorphology is the basis for these angle expression differences.
The Schreger Pattern is a shadow phenomenon created primarily by the structure of microscopic dentinal tubules (Miller 1890; Miles and White 1960; Miles and Boyde 1961); the contribution of laminar dentine deposition to the Schreger Pattern is suggested but not fully understood. Dentinal tubules are fluid transport microcanals that radiate medially to laterally in rows from the center of the tusk, like the spokes of a wheel. Tubule diameter ranges from approximately 0.8 μm to 2.2 μm, and proboscidean dentinal tubules are sinusoidal. Both mammoth and modern elephant dentinal tubules have peak to peak sinusoidal wave distances of 0.8 to 2.5 mm. The visual perception of the Schreger Pattern is a function of intertubule distances and the wave alternation of adjacent dentinal tubule rows.
Scanning electron microscopic examinations of Loxodonta, Elephas, and Mammuthus ivories revealed differences in tubule density. Tusks with effectively equal macromorphology have more dentinal tubules per unit area in mammoths than in modern elephants (fig. 3).
Fig. 3.
Radial section scanning electron micrographs of (left) Mammuthus primigenius and (right) Loxodonta africana illustrating the tubule density per area difference between extinct and modern proboscidean ivories. Bar equals 10 μm, original magnification 1000 x
 |
The effect of greater tubule density creates shadow lines that form small (acute) Schreger angle patterns such as those seen in mammoth ivory. Fewer tubules per unit area, as observed in Loxodonta and Elephas ivories, result in greater distance between shadows and therefore greater (obtuse) angles (fig. 4).
Fig. 4.
Transverse sections of (left) Mammuthus primigenius and (right) Loxodonta africana ivories showing the acute angle Schreger Pattern angles in Mammuthus and obtuse Schreger Pattern angles in Loxodonta. Bar equals 1 cm
 |
The Schreger Pattern is a unique and reliable identifier of proboscidean ivory. Statistical analysis and microscopic observations show that the Schreger Pattern can also serve to nondestructively and objectively differentiate between elephant and mammoth ivories.
ACKNOWLEDGEMENTS
The authors thank Larry Agenbroad, William Gould, Clayton Ray, and Richard Tedford for contributing mammoth ivory standards used in this study. We also thank Bernhard Binder, Evelyn Burchett, and Susan Taylor and for translations of the Schreger and Obermayer papers, and Stephen D. Busack for critical review of this manuscript.
|