CHEMISTRY AND CONSERVATION OF PLATINUM AND PALLADIUM PHOTOGRAPHS
ADAM GOTTLIEB
3 RE-CREATING THE PALLADIUM PRINTING PROCESS
3.1 METHODOLOGY
On the basis of this list of chemicals, the palladium printing process was re-created. To minimize contamination, materials free of metal parts were chosen for all contact with chemicals and prints; these include measuring spatulas, containers, print frames (except for hinges), trays, tongs, and clothespins.
Articles dating from the 19th century suggest that between 1.8 and 3.0 parts of iron (III) should be used per part of platinum(II) or palladium(II) (Pizzighelli and von Hübl 1886). Solutions of ferric oxalate and sodium tetrachloropalladite were prepared as follows, so that equal amounts would give 2.4 parts of iron(III) per part of palladium(II).
Ferric oxalate solution was prepared by disolving 24.8 g in distilled, deionized water to 100 ml final volume. Traditionally, about 1.7 g of oxalic acid are added to the ferric oxalate solution, and two solutions of ferric oxalate are prepared, to one of which 0.46 g of potassium chlorate are added. Oxalic acid was not used. In order to permit the maximum number of variables to be studied independently, potassium chlorate was prepared separately in 3% by weight solution rather than added to the ferric oxalate solution (see section 3.4.2). A coating of 22 drops ferric oxalate–potassium chlorate solution for use with low-contrast negatives, standard in modern platinum printing manuals, is replaced by 20 drops ferric oxalate solution plus 6 drops potassium chlorate solution. Sodium of tetrachloropalladite solution was prepared by dissolving 9.5 g palladious chloride dihydrate plus 8.3 g sodium chloride in distilled, deionized water to a final volume of 100 ml.
Crane's Kid Finish cotton rag paper was used. For the test discussed in section 3.4.1, the paper was sized prior to sensitization. The coating employed, except for the tests discussed in sections 3.4.2 and 3.4.3, consists of 20 drops ferric oxalate solution plus 4 drops potassium chlorate solution plus 20 drops sodium tetrachloropalladite solution. The drops are swirled together, poured along one edge of a sheet of paper, and spread across the paper by rolling with a glass rod. The paper was coated once, allowed to dry, and then coated again starting from the opposite end to make an even coat. If, upon inspection, the coating appeared to be uneven, another piece of paper was coated. For the test discussed in section 3.4.1, only one coating was possible. Only one final print was made for each level of each control variable; thus statistical validity of the results cannot be shown.
Coated paper was exposed by contact-printing with up to 12 identical 120- format negatives in a single contact print frame. Exposure was therefore identical for all prints within a test group, except for the tests discussed in sections 3.4.3 and 3.5.1. The exposure unit consisted of 12 20 W fluorescent ultraviolet-emitting bulbs, a total of exposure of 240W. After exposure, the paper was cut up into its individual images, which were then subjected to different treatments depending on the variable being tested.
Developers were prepared with distilled, deionized water; fixers, with tap water. Prints within a given test group were developed simultaneously or in quick succession, as soon after exposure as possible. They were developed for 3 minutes at 70°F, and cleared for 3 minutes in each of three baths of 1:199 hydrochloric acid. Cleared prints were rinsed together for 10 minutes in running tap water and then hung up together to air-dry on a line. Upon drying, all prints within a test group were sealed together in a plastic bag, which in turn was sealed in a light-tight plastic bag stored in a darkroom. Prints were stored in this way until they could be analyzed and again after analysis.
Prints were analyzed visually for tone, shadow density, grain size, and contrast. In many cases, differences were very subtle and difficult to interpret. In general, wherever prints do not have comparable shadow density, contrast is extremely difficult to assess for lack of a common reference point. Lower highlight density exaggerates the already warm or cold tone of a print.
Effects on contrast, grain size, and tone are extremely difficult to assess when bleaching occurs. Bleaching increases contrast and reduces shadow density. It also appears to make palladium prints grainier by making the palladium deposite less even, and warmer by removing density from the shadows. None of these variables is affected when bleaching does not occur. Thus, for tests in section 3.3, all apparent effects of the bleaching clearing agents citric acid, hydrochloric acid, and oxalic acid are discounted.
3.2 DEVELOPING
3.2.1 DIFFERENT DEVELOPERS
In contrast both to developers for silver prints and to sensitizers and toners for platinum prints, knowledge of the wide variety of developers for platinum and palladium prints has not survived in the modern literature. Present-day platinum printing manuals discuss only three kinds of developers: those based on potassium oxalate; those based on sodium acetate, and those based on citrates (Sullivan 1992; Steinberg 1992; Nadeau 1986; Shillea 1986; Hafey and Shillea 1979; Rexroth 1977). Many of the developers that have disappeared from the platinum printing literature remain inexpensive and available. As a group, they permit extensive control over print contrast and tone and required exposure time.
Nine of the most popular developers from the late 1800s were tested (table 1). Dilution formulas for single-compound developers other than potassium oxalate do not exist in the literature of the time. Thus, weight-equivalent solutions of the standard oxalate developer, 454 g to 1420 ml final volume in water, or 1.67M, were prepared.
TABLE 1 DEVELOPERS TESTED
Effects of different developers on contrast, tone, and shadow density are difficult to assess when hydrochloric acid is used as a clearing agent, as is discussed in section 2.1. Therefore, a second set of tests was performed with a nonbleaching clearing agent, tetrasodium ethylenediaminetetraacetate (EDTA tetrasodium). However, here tone cannot be compared in all cases because EDTA tetrasodium dramatically alters the color of prints processed in basic developers.
CONCLUSIONS: The developers tested (see table 1) can be grouped roughly into the following categories: warm-toned: 2, 3, 7; warm- to neutral-toned: 4, 5, 8; neutral- to cold-toned: 1, 6; weak: 2, 6, 7, 9; high-contrast: 1, 6, 8; low-contrast: 2, 7. Prints developed in potassium carbonate, sodium carbonate, monohydrate, or sodium phosphate dibasic heptahydrate become orange in tone when cleared with EDTA tetrasodium.
3.2.2 TEMPERATURE OF DEVELOPER
Room-temperature developers have long been standard in photography. Their advantages over hot developers include ease of use and lower volatility, so they are less toxic. Platinum printing was created as a hot-developer process. Many years later it became a cold-bath process like palladium printing (seesection 2.1). In modern platinum printing practice, a developer is heated only to increase its activity with a view to salvaging an underexposed print or to give prints a warmer tone. As the added density is not nearly proportional to the increase in temperature, the former is not a powerful remedy. Some sources indicate that sodium carbonate will work as a developer only when hot.
Ammonium citrate, potassium oxalate, and sodium carbonate were each tested at 40, 70, 110, and 180°F (fig. 1).
Fig. 1.
Prints showing the effects of varying developer temperature. Key: 1. ammonium citrate 40°F; 2. ammonium citrate 70°F; 3. ammonium citrate 110°F; 4. ammonium citrate 180°F; 5. potassium oxalate 40°F; 6. potassium oxalate 70°F; 7. potassium oxalate 110°F; 8. potassium oxalate 180°F; 9. sodium carbonate 40°F; 10. sodium carbonate 70°F; 11. sodium carbonate 110°F; 12. sodium carbonate 180°F
 |
CONCLUSIONS: The most dramatic change that occurs as developer temperature is increased is warming of print tone. This change in behavior is best illustrated by ammonium citrate: it produces cold-toned prints at 40°F and warm-toned prints at 180°F. Potassium oxalate produces warm tones at all temperatures but especially at 180°F. In both cases, contrast decreases slightly with increasing temperature, while shadow density increases slightly. Sodium carbonate exhibits the same behavior as the other two developers up to between 70 and 110°F. Above this range prints begin to develop a yellow tone. Finally, at 180°F, sodium carbonate nearly blackens prints owing to the formation of insoluble ferrous carbonate.
3.2.3 DILUTION OF DEVELOPER
As indicated in section 3.2.1, dilution formulas for developers other than those based on potassium oxalate do not exist in the literature. At a concentration of 1.67M, the standard potassium oxalate developer is exceedingly strong by silver photography standards. Use of potassium oxalate at this concentration or other developers in weight-equivalent solution is not economical and may not be necessary.
Potassium oxalate, sodium acetate, and sodium carbonate were each tested at 0.05, 0.30, 0.83, and 1.67M concentration.
CONCLUSIONS: Potassium oxalate produces black shadows at as low a concentration as 0.30M. It becomes only slightly stronger as concentration is increased thereafter. Sodium acetate does not produce vigorous images below a concentration of 0.82M; its performance improves significantly with increased concentration. Both developers become colder in tone and higher in contrast as they are diluted.
3.2.4 ACIDITY OF DEVELOPER
Early sources recommend acidifying potassium oxalate developer with oxalic acid to prevent the formation of basic iron salts, which give prints a yellow tone (Pizzighelli 1883). It is now common practice to use oxalic acid in the sensitizer instead. However, with a citrate developer it would be more appropriate to use citric acid, whether in the sensitizer or in the developer. Excessive acidification of the developer may carry the danger of bleaching prints, by causing developer acidity to approach that of a clearing bath.
Ammonium citrate was tested with 0, 2, 12, 40, and 100 g/L citric acid added. Potassium oxalate was tested with 0, 1, 6, 20, and 50 g/L oxalic acid added.
CONCLUSIONS: Addition of any reasonable amount of oxalic or citric acid to potassium oxalate or ammonium citrate developer, respectively, will not affect prints in a visible way for developing times of 3 minutes or less. Since a clearing solution of 5% citric acid will begin to bleach prints visibly after between 9 and 24 minutes, some bleaching will occur if a print is immersed for that length of time in a citrate developer containing 50 g/L citric acid (see section 3.3.3). The same result occurs for developing times of 3 minutes or more in an oxalate developer containing 12.5 g/L oxalic acid.
3.2.5 DEVELOPING TIME
A characteristic of platinum printing cited in almost all of the literature is that it is impossible to overdevelop an exposed print. Beyond a certain point, a developer may bleach a print more than it continues to add density.
Ammonium citrate and potassium oxalate were each tested for 0.5, 2, 6, and 20 minutes developing time.
CONCLUSIONS: Exposed paper processed in either 1.67M potassium oxalate or 1.67M ammonium citrate will be completely developed after 30 seconds. No changes in contrast or shadow density will be observed with ammonium citrate for developing times up to 20 minutes. Potassium oxalate will very slightly decrease contrast and shadow density with increased developing time.
3.2.6 COMBINED EFFECTS: DEVELOPER DILUTION AND DEVELOPING TIME
This test was performed to determine the minimum developer dilution and time required to produce complete development when using potassium oxalate.
Dilution and developing time were cross-tested at 0.05, 0.30, 0.82, and 1.73M, and 1, 3, and 8 minutes, respectively.
CONCLUSIONS: Developing in potassium oxalate is complete for developing times greater than 30 seconds at a concentration of 0.30M or stronger. Potassium oxalate in 0.05M solution will not adequately develop prints for any developing time up to 8 minutes. Potassium oxalate will bleach prints at a concentration of 0.05M or higher.
3.3 CLEARING
There are two important considerations in the choice of clearing agent, clearing time, and clearing agent dilution. The first is permanence. The clearing agent must be strong enough and prints immersed long enough so that all iron salts are removed. Unexposed ferric oxalate will darken with further exposure to light and will in time both fog and stain a print; uncleared ferrous oxalate will also stain a print.
The second consideration is bleaching. Whereas platinum is not susceptible to bleaching, palladium is partially dissolved by acid (see section 2.1). Among traditional clearning agents, significant bleaching can occur with hydrochloric acid. Bleaching increases the required exposure time and, more important, gives prints a splotchy appearance. Whether a dilution is too strong or a clearing time too long is different for each clearing agent.
3.3.1 DIFFERENT CLEARING AGENTS
Three clearing agents have been used almost exclusively in the history of platinum and palladium printing: hydrochloric acid, oxalic acid, and citric acid. The first is by far the most common. Oxalic acid is rarely mentioned in current manuals. Many commercially available palladium printing kits now use EDTA tetrasodium, a nonbleaching clearing agent.
Different clearing agents cannot be compared on a simple basis, as developers can. The extent to which bleaching clearing agents will bleach prints depends on the dilution in which they are used and on the length of time for which a print is cleared. Conversely, the variables of time and dilution are almost absent in developing: overdeveloping is impossible, and most developers behave similarly with dilution. Therefore, a test like that performed in section 3.2.1, where different developers were compared, is inconclusive here. This section simply lists different clearing agents that have been used in platinum and palladium printing, together with the dilutions in which they are conventionally prepared (table 2).
TABLE 2 CLEARING AGENTS TESTED
3.3.2 DILUTION OF CLEARING AGENT
Prints were cleared for 3 minutes in each of three baths. Citric acid was tested in 1:19, 1:49, 1:99, and 1:249 dilution. EDTA tetrasodium was tested in 1:22, 1:44, 1:99, and 1:333 dilution. Hydrochloric acid was tested in 1:49, 1:149, 1:399, and 1:999 dilution. After rinsing and drying were complete, prints were exposed for 48 hours to ultraviolet light from a 240W exposure unit, to determine how well cleared they were. This procedure is primitive and does not indicate how the prints will behave over a long period. The result, given here and in section 3.3.4, that all prints appear to have been properly cleared, is not conclusive. Facilities for studying accelerated aging of photographs are required if a better assessment is to be made.
CONCLUSIONS: For 3 minutes of clearning in each of three baths, or 9 minutes total clearing time, only hydrochloric acid in solutions stronger than between 1:49 and 1:149 dilution will bleach prints. Neither citric acid nor EDTA tetrasodium will bleach prints when used in up to 2.5 and 3 times standard concentration, respectively, for this amount of time. All prints were properly cleared.
3.3.3 CLEARING TIME
Standard dilutions of each clearing agent were used. Citric acid, EDTA tetrasodium, hydrochloric acid, and oxalic acid were each tested for 1, 3, 8, and 20 minutes in each of three baths, or 3, 9, 24, and 60 minutes total. Prints were not tested for proper clearing.
CONCLUSIONS: Except for oxalic acid, which bleaches significantly when used for more than between 3 and 9 minutes, clearing agents used in standard dilution produce almost no bleaching. Among the three remaining clearing agents, hydrochloric acid bleaches slightly more than citric acid, and citric acid bleaches slightly more than EDTA tetrasodium, which does not bleach. Extensive bleaching occurred only upon 60 minutes of clearing in 1:149 hydrochloric acid.
3.3.4 COMBINED EFFECTS: CLEARING AGENT DILUTION AND CLEARING TIME
This test was undertaken in order to determine the optimal clearing agent dilution and clearing time for clearing prints thoroughly without bleaching when using a bleaching clearing agent. The test was performed with hydrochloric acid. After clearing, washing, and drying were complete, prints were exposed for 48 hours to ultraviolet light from a 240W exposure unit to determine how well cleared they were.
Dilution and clearing time were cross-tested at 1:49, 1:149, 1:399, and 1:999, and 1, 3, and 8 minutes per bath, or 3, 9, and 24 minutes total, respectively (fig. 2).
Fig. 2.
Prints showing the effects of varying clearing agent dilution and clearing time. (Test performed with hydrochloric acid.) Key: 1. 1:49 dilution, 3 minutes; 2. 1:49 dilution, 9 minutes; 3. 1:49 dilution, 24 minutes; 4. 1:149 dilution, 3 minutes; 5. 1:149 dilution; 9 minutes; 6. 1:149 dilution, 24 minutes; 7. 1:399 dilution, 3 minutes; 8. 1:399 dilution, 9 minutes; 9. 1:399 dilution, 24 minutes; 10. 1:999 dilution, 3 minutes; 11. 1:999 dilution, 9 minutes; 12. 1:999 dilution, 24 minutes
 |
CONCLUSIONS: Hydrochloric acid will bleach prints noticeably when used in 1:49 dilution for 3 minutes total clearing time or longer. In 1:149 dilution, it will bleach prints very slightly when used for more than between 9 and 24 minutes. Bleaching action stops at weaker than between 1:149 and 1:399 dilution for total clearing times of 24 minutes or less. Remarkably, a developed print immersed in 1:999 hydrochloric acid for only 3 minutes will be properly cleared.
3.4 ADDITIVES
Additives—small amounts of chemicals that are not essential to the functioning of the platinum and palladium printing process—provide a direct and radical way to affect image contrast, image tone, and paper sensitivity.
Many additives that were popular while the chemistry of platinum printing was being developed, particularly the heavy metal salts lead nitrate, mercuric chloride, and uranyl nitrate, are highly toxic as well as now expensive or difficult to obtain.
The main drawback of most inorganic additives is that once they have been used, brushes, trays, and solutions become instantly if often imperceptibly contaminated. With the exception of aluminum potassium sulfate (alum), chromic potassium sulfate (chrome alum), and sodium carbonate, sizings that have been used with platinum paper are organic and will not interfere with the chemistry of the process.
3.4.1 SIZING
In the 19th and early 20th centuries paper to be used for platinum and palladium printing had to be sized. Sizing prevents the sensitizer from penetrating the paper fibers too deeply, thus yielding a weak image and wasting expensive palladium or platinum. As most papers today are sized by the manufacturer, sizing is now rarely necessary. Nonetheless, sizing affords surprisingly subtle control over image tone.
Three sizing agents have commonly been recommended for platinum and palladium printing: arrowroot, gelatin, and gum arabic. Each was tested. Sizing instructions usually call for the addition of a small amount of ethanol to speed drying. This method is optional and might affect image tone; it was not used. Gelatin solution is strained before using.
Sizing dilutions were arrived at through experimentation: solutions were prepared as concentrated as they could be without making an uneven coat. The concentrations used were arrowroot, 1.4% (w/v); gelatin, 0.66% (w/v); gum arabic, 15% (v/v). Paper was soaked in, rather than coated with, dilute solutions of sizing agent, and sized twice. Between coatings, paper was hung up and allowed to air-dry.
CONCLUSIONS: Among the sizing agents tested, gelatin and gum arabic will affect prints noticeably in the concentration used. Both increase highlight and shadow density equally and so lower contrast; gum arabic also gives prints a slightly warm tone. All effects appear to result from coloration of the paper by the sizing agent rather than from a change in the metal deposit.
3.4.2 ADDITIVES TO SENSITIZER
It is now standard practice to control contrast in platinum and palladium prints by means of additives to the sensitizer. Potassium chlorate is used almost exclusively for this purpose. Many years ago, potassium chlorate in the sensitizer was complemented by potassium dichromate in the developer. Modern platinum and palladium printing manuals consulted say that potassium dichromate cannot be use in palladium printing, as it will cause the image to be bleached upon clearing (Rexroth 1977; Shillea 1986). By contrast, potassium dichromate is mentioned for use specifically with palladium prints by the British Journal of Photography on three occasions (1918a, 1918b, 1921). Both potassium and sodium dichromate were tested as replacements for potassium chlorate in the sensitizer; the literature indicates that counterions other than dichromate will produce different tones. Powdered dichromates are extremely toxic.
Two related and milder oxidants, potassium chromate and potassium bromate, were also tested, as potassium nitrite, which can function as either an oxidizing or a reducing agent and is mentioned in the literature as a developer additive when processing stale paper.
These oxidants are analogous to restrainers in silver chemistry: they increase contrast, lengthen required exposure time, and affect print tone. In platinum and palladium printing, contrast control agents also serve to keep ferric oxalate from being reduced by platinous and palladious chlorides prior to exposure. In the 19th century, toning agents were often incorporated into the sensitizer. Mercuric chloride, for example, was used in commercial sepia platinum papers. These were not tested.
For the reason outlined in section 3.1, solutions were prepared weight-equivalent to 3% (0.24M) potassium chlorate, as follows: potassium bromate, 4.1%; potassium chromate, 4.8%; potassium dichromate, 7.2%; potassium nitrite, 2.1%; sodium dichromate dihydrate, 7.3%. Each additive was tested at 2 drops per coat. Potassium chlorate, potassium dichromate, and potassium nitrite were each further tested at 0, 1, 4, 7, and 12 drops per coat, 6 drops corresponding to the upper limit recommended by current manuals (see section 3.1). In the latter test, comparison among additives is not possible, as the exposure times that were required to enable comparison within each additive's series are different (fig. 3).
Fig. 3.
Prints showing the effects of varying sensitizer additives and the concentration of the additives. Key: 1. potassium bromate, 2 drops; 2. potassium chlorate, 0 drops; 3. potassium chlorate, 1 drop; 4. potassium chlorate, 2 drops; 5. potassium chlorate, 4 drops; 6. potassium chlorate, 7 drops; 7. potassium chlorate, 12 drops; 8. potassium chromate, 2 drops; 9. potassium dichromate, 0 drops; 10. potassium dichromate, 1 drop; 11. potassium dichromate, 2 drops; 12. potassium dichromate, 4 drops
 |
CONCLUSIONS: Of the six additives tested, only potassium chlorate, potassium dichromate, and sodium dichromate are useful for controlling contrast. These additives raise contrast while requiring longer exposure time. When the other three additives tested are used, black shadows cannot be obtained even by overexposure. There was no visible difference in the behaviors of potassium and sodium dichromate. Potassium bromate and potassium chromate are too weak to affect contrast appreciably. Potassium nitrite decreases both contrast and required exposure time and so functions as a reducing agent; it may also make prints cooler in tone. Potassium chlorate has a weaker effect on contrast and exposure time than do the dichromate salts. Remarkably, in contrast to the findings of Shillea (1986), neither potassium chlorate nor either of the dichromates will produce visible graininess when used to excess, up to 12 drops of 0.24M solution. When more than between 4 and 7 drops of either solution are used, even very long exposure times may fail to produce black shadows. Use of dichromate salts in the sensitizer will not cause palladium prints to be bleached upon clearing in hydrochloric acid.
3.4.3 ADDITIVES TO DEVELOPER
Only for the past 50 years has it been standard practice to use contrast-control additives exclusively in the sensitizer. The obvious benefit is that the contrast of an individual print can be controlled more finely while prints prepared and processed alongside it remain unaffected. In the long term, however, additives to the sensitizer will accumulate as an impurity in the developer. Conversely, by using contrast-control agents in the developer, paper that has already been coated can be contrast corrected. These additives can be used to prepare a series of developer having different contrast, much like having graded papers.
The same factors apply to toners and intensifiers in the developer. Given that these are more expensive than contrast control agents, and that it is more wasteful to use additives in the developer than in the sensitizer, their use is costly. Nonetheless, adding just enough toner or intensifier to the developer for one print should not be wasteful. Toners and intensifiers were not tested.
Additive solutions were prepared as in section 3.4.2. Potassium chlorate, potassium dichromate, and potassium nitrite were each tested at 0, 1, 8, and 50 drops per L of potassium oxalate developer.
CONCLUSIONS: The addition of as few as 8 drops of either 3% potassium chlorate or 7.2% potassium dichromate solution to 1 L of standard potassium oxalate developer may visibly raise contrast in a print. The effect remains so subtle that there is no substantial increase in required exposure time when up to 50 drops of additive are used. Potassium nitrite does not have any visible effect at the concentrations tested. The use of potassium dichromate in the developer does not cause bleaching.
3.4.4 TONER AND INTENSIFIER
The only way to change an individual print without at all affecting the chemicals used to process other prints is to tone or intensify it after clearing. While this procedure is not as economical as adding toning agents to the sensitizer, it affords more control because the toning process can be stopped at the desired moment.
A great many toners and intensifiers for platinum and palladium prints were used in the 19th century. As mentioned in section 3.4, most are extremely toxic. The relatively safe toners (gold chloride and ferric ammonium sulfate) and intensifiers (silver nitrate, potassium tetrachloroplatinite, and sodium tetrachloropalladite) require special solvents, developers, and clearing agents, many of which in turn are either mildly or highly toxic. Cupric chloride, a toner used in either the developer or clearing agent, is relatively safe. A toner test was not performed.
3.5 STORAGE
Due to stability problems associated with the paper base, platinum printing has turned out to yield far less permanent photographs than was thought or hoped. The state of old platinum and palladium prints is now of great concern. Investigation into why and how platinum prints deteriorate has been based exclusively on the study of existing prints, most of them several decades old (Rempel 1987; Reilly 1986; Flieder 1985; Norris 1985). The tests described below offer additional insights into the impermanence of platinum and palladium prints.
Unexposed and exposed but unprocessed platinum paper must be stored very carefully, especially the former. Over long periods of time finished platinum and palladium prints also deteriorate. In each case, the envisioned enemies of permanence are moisture, heat, and ultraviolet light. In the case of finished photographs, decay of the paper is also a factor. The decay chemistry peculiar to platinum prints may be related to the handling of the paper before exposure and before processing. Mishandling a platinum print in these stages may visible signs of decay much more rapidly than it will once the print is finished.
To test the often conflicting literature as to how platinum and palladium paper should be handled, the behavior of unexposed and exposed but unprocessed palladium paper was tested over a period of 12 days in a room-temperature, light- and air-tight, but not humidity-controlled, environment.
3.5.1 UNEXPOSED PAPER
Paper was coated, stored for a set period of time before it was exposed, and then processed immediately following exposure. Storage times tested were 0, 1, 6, 18, 48, 96, 168, and 288 hours, measured from the moment paper dried after coating.
CONCLUSIONS: Coated paper that is stored before exposure decreases gradually in contrast. Specifically, shadow density decreases slightly, while highlights darken. This effect begins to be noticeable after between 1 and 6 hours of storage.
3.5.2 EXPOSED BUT UNPROCESSED PAPER
Paper was coated, exposed immediately upon drying, and then stored for a set period of time before it was processed. Storage times tested were 0, 1, 6, 18, 48, 96, 168, and 288 hours, measured from the moment exposure was complete (fig. 4).
Fig. 4.
Prints showing the behavior over time of exposed but unprocessed paper. Key: 1. 0 hours storage; 2. 1 hour storage; 3. 6 hours storage; 4. 18 hours storage; 5. 48 hours storage; 6. 96 hours storage; 7. 168 hours storage; 8. 288 hours storage.
 |
CONCLUSIONS: Paper that is stored between exposure and developing increases dramatically in contrast and grain size. Both effects begin to be visible after between 1 and 6 hours of storage. In terms of contrast, shadow density remains constant, while highlights lighten significantly.
This effect begins to reverse, however, after between 4 and 7 days of storage. While grain size does not change, contrast decreases significantly: highlights darken and shadows lighten. Paper that is stored unexposed exhibits the same behavior.
3.5.3 PROCESSED PAPER
Finished photographs have been far more extensively studied than either unexposed or exposed but unprocessed platinum and palladium papers, yet it is in the later group that long-term deterioration of prints can be observed. In most reports, the cause of deterioration of the photograph has been found to be decay of the paper, not of the image. Reilly (1986) cites the following factors: chemicals, notably iron salts and acid, already in the processed paper; the catalytic properties of platinum and to a lesser extent palladium; the absence of a binder layer; the quality of the paper; and exposure to light and chemicals during storage and exhibition. Similar information appears in Rempel (1987), Flieder (1985), and Norris (1985).
|