METHODS AND MATERIALS FOR FILLING LOSSES ON LACQUER OBJECTS
MARIANNE WEBB
ABSTRACT—Whether the infilling of losses on lacquer is done for purely structural or aesthetic reasons, appropriate methods and materials vary widely. Because the materials of lacquer itself differ from East to West, the article is divided into two parts: fills for Asian lacquer and fills for Western lacquer.Over the past few centuries many materials have been used to fill losses in lacquer: Asian lacquer, wax, polyester, poly (vinyl acetate), epoxy, gesso, acrylic paints, acrylic resins, formulations of synthetic polymers such as Polycite, as well as the traditional materials of shellac and other natural resins. The benefits and disadvantages of each are outlined. Bibliographic references from numerous publications on the subject have been collected for this article.
TITRE—Méthodes et matériaux pour compenser les pertes sur des objets laqués. RÉSUMÉ—Les matériaux utilisés pour compenser les pertes dans la laque et leur méthodes d'application varient grandement, que la réparation soit effectuée pour des raisons purement structurelles ou bien esthétiques. En raison des différences qui existent entre la laque produite en Asie et celle produite en Occident, cet article est divisé en deux parties qui traitent des matériaux séparément, en fonction de leur origine.Au cours des derniers siècles, on a utilisé de nombreux matériaux pour combler les lacunes de laque: laque d'Asie, cire, polyester, epoxyde, plâtre, alcool polyvinyle, peinture ou résines acriliques, mélange de polymers synthétiques comme le Polycite, et des matériaux traditionnels comme la gomme-laque et autres résines naturelles. Les avantages et inconvénients de chacun de ces matériaux sont décrits. Des références bibbliographiques provenant de nombreuses publications sur le sujet sont rassemblées à la fin de l'article.
TITULO—Métodos y materiales para rellenar pérdidas en objetos de laca. RESUMEN—Aún cuando la reposición de faltantes en lacas se haga por razones puramente estructurales o estéticas, los métodos y materiales apropriados varían ampliamente. Debido a que los materiales de la laca difieren de este a oeste, el trabajo se dividió en dos partes, rellenos para lacas asiáticas y rellenos para lacas occidentales.En los siglos pasados muchos materiales han sido utilizados para reponer faltantes en lacas; laca asiática, ceras, polyester, epoxy, yeso, alcohol polivinílico, pinturas acrílicas, resinas acrílicas, fórmulas de polímeros sintéticos como el Polycite, y materiales tradicionales como el shellac y otras resinas naturales. Se reseñan los beneficios y desventajas de cada uno de estos materiales. Para este artículo se recolectaron referencias bibliográficas de numerosas publicaciones sobre el tema.
1 INTRODUCTION
Whether the lacquer artifact is a study piece or of prime importance, adding material to the original is not to be undertaken lightly. It may not be necessary to fill in a loss if the surrounding area is stable and the edges are not exposed. But if the edges are friable, infill is essential to protect the object from losses and further damage. A fill can help maintain the integrity of the surface as well as improve the aesthetics. Often filling in losses helps to improve the viewers' understanding of the piece as well.
For lacquer infills, the first consideration is the type of lacquer. Asian lacquer, known as urushi in Japanese, is quite different from the myriad of resins used to produce European and American lacquer, also known as japanning. Because these two materials are often misidentified, it is important that they be distinguished and treated appropriately. This article is divided into two parts: fills for Asian lacquer and fills for Western lacquer. When the material is unknown, chemical analysis should be under taken prior to commencing treatment (Derrick et al. 1985; Jaeschke 1994).
Throughout this article many Japanese terms have been used. Naturally other Asian languages have their own terms for the fabrication and restoration of lacquerware. The Japanese terms selected for this article have been due to the author's personal experience in Japan and the recent availability of English translations of Japanese literature on lacquerware.
2 FILLS FOR ASIAN LACQUER
2.1 CHARACTERISTICS TO BE CONSIDERED DURING TREATMENT
The two main agents of deterioration of Asian lacquer are light and relative humidity, although temperature also plays an important role. Lacquer falls into the same category as blue wool standard 4. That is, lacquer can be displayed for 40 years at 100 lux or 80 years at 50 lux (UV excluded and 8 hours display per day) before damage will be physically evident. As the surface of light-damaged lacquer may be soluble before a visible change has taken place, extra precautions must be taken when handling. Since aqueous substances cause discoloration, lacquer should be exposed to water only if tests show that it is not damaged by water. Test swabbing should be carried out in areas that have received the maximum exposure to light, not the underside of the artifact. Nonpolar solvents are safest for use with lacquer.
There is evidence that lacquer exposed to a combination of heat and moisture undergoes a thermochromatic change. The author has observed this color change at temperatures as low as 50°C. Therefore heat must be used with extreme caution during treatment.
Lacquerware is also susceptible to damage from fluctuating relative humidity. A decrease in RH can cause a wooden core to shrink, causing stress between it and the inflexible lacquer surface. Cracks will form in the lacquer to relieve the stress. If lacquer is exposed to cycles of low and high relative humidity, the lacquer will eventually start to flake off its wooden core. Sometimes the wooden core will shrink permanently and the lacquer surface will no longer lie flat. During treatment as well as storage and display, it is important not to let the relative humidity drop too low or fluctuate wildly. A stable relative humidity of 50–60% is recommended.
Asian lacquer is often coated onto a number of substrates and grounds. Not all ground layers are a durable lacquer-based variety. In many cases they are a water-soluble animal glue mixed with clay or another inert material. This material can also contribute to the deterioration of the object, and its sensitive nature must be taken into account during treatment. A number of water-soluble methods are discussed below, and all must be used with caution to ensure that further damage does not occur. Due to the variety of grounds in use and the mostly organic materials of the substrate, relative humidity should remain stable during storage, treatment, and display.
2.2 ASIAN LACQUER (URUSHI)
Assuming the need for a fill has been established, what are the materials available to the modern conservator? A natural choice might be to fill the loss with the same material as the original. In the case of Asian lacquer, this choice might not be suitable or practical for most Western conservators. Asian lacquer is difficult to work with, and excellent results are hard to achieve. It takes years of training to be able to select the appropriate mixture for consolidation and infilling. Even satisfactory results might be unlikely for the typical Western-trained object conservator, because the application technique is as important as the material itself.
There are additional factors to consider as well. For most practical purposes, Asian lacquer is an irreversible medium; it cannot be dissolved with solvents, although fills can be picked out with a scalpel. Additionally, lacquer fills are difficult to color-match and over time will change color at a rate different from that of the original, producing an increasingly mismatched fill. Moreover, many conservators consider it of prime importance to use fill materials that are not the same as the original so that the restoration can never be mistaken for the original.
The above notwithstanding, there is a growing body of literature written in English that outlines the procedures for filling with Japanese urushi (Arai 1985; Nakajima 1985; Konishi 1993; Piert-Borgers 1993; Murose 1996). Throughout these articles the general theme is the same: repairs are done in the same manner as the original object was made, and each layer lost is repaired with the same material as the original. In the case of objects that were originally created with many layers, infills are often simplified to a few layers. When fills are not done, the remaining ground is consolidated with raw urushi. As always, each object is considered on an individual basis (Yamashita 1995).
While it is unlikely that any of the methods described below will be used by Western conservators, they are explained to aid in recognizing the previous repairs. Many pieces now in U.S. or Canadian collections were repaired in the traditional methods prior to leaving Asia.
Kokuso, a mixture of urushi, baked sawdust, and flour (Kitamura 1985), is commonly used as a fill material on sculpture and other large wooden objects (Onodera 1982). It is used primarily for deep cracks and losses to the foundation layer. In Japan, many conservators have adapted the standard kokuso recipe to best suit their own needs. Usually, mugi urushi is made first by mixing flour and water into a paste and adding the urushi slowly, then finally adding the sawdust to make kokuso. Variations include the addition of nori urushi (rice flour and urushi) or chopped linen fibers. Depending on the amount of urushi in the mixture, the final fill may vary in color from beige, containing little urushi, to dark brown.
Although the basic mix of sabi is raw urushi and tonoko (pulverized baked clay), there are many subtle variations on this recipe and its appearance. The clay may vary in color from dark gray to beige depending on its origin. A great many grinds are available for use, including the coarser baked clay known as jinoko, although it is used infrequently for repairs.
The final finishing layers over the ground must be the right type of refined urushi. Conservators in Japan often spend a great deal of time achieving the proper combination to blend with original surface. Even a cursory examination of the materials and methods of repair confirms the complexity of these repair techniques.
2.3 WAXES
Wax is a common fill material that has been used successfully for many different types of restorations in the past. Indeed, even the Romans used it to repair Greek marble statuary broken during transport. Marbles that had not been repaired with wax were marked sine cere (without wax), hence our word “sincere.” Some conservators contend that lacquer fills should also be marked sine cere, because wax restorations can cause problems for future conservators.
Although the literature documents a number of successful treatments involving wax, there are a great many concerns about its use. Asian conservators point out that wax residues may make it impossible for them to do a subsequent urushi repair. Much discussion has taken place on whether the wax inhibits the urushi drying process and causes additional cracking (Nakajima 1985). An experiment by Piert-Borgers (1993) shows recently applied beeswax does not affect the drying of urushi, but there may be problems with unknown wax formulations or aged wax surfaces.
There is also the consideration of whether wax is truly reversible. In theory it is, but in practice removing all traces of the wax from the ground layers without harming the object is just about impossible. Once wax has been introduced to the porous ground layers, the choice of subsequent treatments is severely limited. Any fill area where wax is used should be lined with Paraloid B-72 before filling to ensure that the wax does not enter the ground layers. The author now restricts the use of wax to objects where small losses, less than 1 cm in diameter, occur in areas of thick lacquer, .318 cm or more, such as on Chinese carved lacquerware.
At the Royal Ontario Museum, extensive use of wax was made for the infilling of losses on a namban lacquer chest in 1984. At the time, wax seemed suitable for this project since the fill areas between the mother-of-pearl were small and the urushi layers were fairly thick. A combination of beeswax and carnauba with vine black pigment was used for infilling the numerous losses at the edges of the cabinet. The wax was first heated, pigment added, and then allowed to cool into colored wax blocks. A hot stylus for batik wax was used to melt the wax and guide the flow into the loss. The small fill areas on this object were easy to smooth out with odorless mineral spirits, but slightly larger areas were problematic.
Although the wax fills appear to have worked quite well in this circumstance, they will not be undertaken again for a number of reasons. Because beeswax corrodes copper, this formula cannot be used near any metal fixtures. Also, unless the beeswax is extremely pure, the wax fills may bloom over time. In the case of this namban cabinet, all the surfaces had to be coated with PVA resin shortly after conservation treatment to prevent blooming. Inpainting was also difficult, as few standard mixtures are compatible with wax (fig. 1).
Fig. 1.
Back panel of Japanese namban cabinet. The lower decorative edge has been restored using a beeswax and carnauba wax mixture. Note the beginning of wax bloom.
 |
The wax mixture that has been used at the Freer Gallery of Art for thick layers of carved lacquer in the past is perhaps a better choice. Chase (1985) reported that after lining the loss with 10% Paraloid B-72, a mixture of 38% carnauba, 38% paraffin wax, and 10% microcrystalline was used for filling in a Ming dynasty carved dish. When additional tack is needed a resin may be added (Norman and Koob 1994).
Wax has also been used in combination with resin mixtures in Russia. Simonov (1996) reports success with a wax dammar resin mixture used either as a direct fill or as cast sheets that are then cut to shape. He has used the technique of taking a mold of low relief areas, then casting missing areas using Montan wax. He advises that extra caution be taken when applying any hot wax to lacquer, as the lacquer may undergo a color change at around 100°C (Simonov 1990). Those who have seen the dramatic discoloration in lacquer soup bowls are aware of this problem.
In conclusion, the various problems with wax fills—difficulty inpainting, danger of thermochromatic changes, lack of complete reversibility, and the possible effect on the drying of urushi—preclude its use in most cases.
2.4 POLYESTER RESINS
Polyester resin has been used by some conservators for infilling losses in lacquer. It is used successfully to infill losses in glass, another hard glossy material, so it is logical that it should be tried for lacquer.
Since polyester is generally considered an irreversible resin, there are only a few acceptable ways that it can be used on lacquerware. The first involves lining the fill area with a barrier such as a flexible plastic wrap, then pouring in the fill, letting it dry, removing the wrap, and gluing in the fill using a reversible adhesive. The second is casting the polyester separately, then cutting it to fit the shape of the loss. The third is lining the fill with a reversible resin, then casting and finishing the polyester in situ. Each method has its difficulties.
Jackson (1994) has given a detailed description of the working procedure for producing missing pieces of carved lacquer in polyester. She found polyester particularly useful for reproducing the colored layers of lacquer for carving. The cast, layered polyester fills were carved, then polished to match the urushi, and adhered with Paraloid B-72, making them completely reversible.
Jaescheke(1993, 13) gives a very good description of the use of polyester in situ:
The area to be gapfilled was then coated with a layer of Paraloid B-72 (20%) to provide a protective barrier which is readily soluble if the gapfill is to be removed at some later date. The gap was then filled with polyester resin tinted with polyester black pigment and catalyzed with standard peroxide catalyst. The environmental grade of polystyrene was used. This contains some crystic wax, helping to prevent the release of styrene monomer and preventing the formation of a sticky surface when the polyester is in contact with moisture in the atmosphere. The resin sets hard in about 20 minutes, with a slightly dull surface.
She goes on to describe the polishing process for the polyester. Extra care must be taken when polishing this type of fill in situ as it is easy to abrade the adjacent lacquer area. Water should be avoided to ensure that there is no damage to the lacquer or the ground layers. Micro-Mesh cushioned abrasive cloths, available in grades from 1,500 to 12,000, can be used for polishing without the use of a medium.
In 1990 a series of tests for the use of polyester as a fill material were carried out (Webb 1994). The method chosen was to cast polyester sheets, then to cut shapes for insertion into the lacquer. In general this method was not successful. The pure polyester was too brittle for cutting to shape, and bulking materials that softened the final product made it opaque and pale in color so that it no longer matched the lacquer. It would be also difficult to blend the fill with the surrounding lacquer without putting the lacquer in direct contact with the resin.
2.5 POLYVINYL ALCOHOL AND CALCIUM CARBONATE
Some conservators have used polyvinyl alcohol with calcium carbonate for infilling losses in gilding (Hebrard and Small 1991; Thornton 1991). Since it could be applied easily, dried fast, and also could be burnished to a very smooth finish, it seemed a good candidate for use as a fill in lacquer. Sample panels made at the Royal Ontario Museum and cycled several times through humidity changes from 20 to 90% RH showed that the polyvinyl alcohol and calcium carbonate applied to the surface remained intact and adhered to the wooden substrate. A polyvinyl alcohol and whiting fill is readily reversible using only slightly damp swabs.
For use as a fill, polyvinyl alcohol is dissolved in water to make a solution between 6 and 8%. In the past the author has used a low-molecular-weight polyvinyl alcohol with a high degree of hydrolysis because it was readily available. However, Hebrard and Small (1991) suggest that one with a low degree of hydrolysis may have better working qualities. Calcium carbonate is added to the solution until the mixture reaches the desired consistency—a dough for deep fills or a much less viscous consistency for use as a coating. The resulting mixture is thixotropic, which makes it difficult to spread like a traditional gesso. It is best to apply it with a rubber spatula to obtain a smooth finish in the first attempt. It can be wetted again later for further smoothing but should be dry-sanded for the final finish. Conservators who are accustomed to working with traditional gesso often have difficulty adapting methods to this product, but with practice a very smooth surface can be achieved in a relatively short time.
Some conservators have expressed concerns about using this water-based material with urushi. However, to date the author has not seen any effect on the surrounding urushi of the small amount of water necessary to apply this material or to reverse it. As with any fill material, care must be taken not to expose the surface of the urushi to this material. Another concern is that polyvinyl alcohol cross-links in ultraviolet light. Used in this way, however, this material is not exposed to light.
At the Royal Ontario Museum this fill material was first used for the extensive losses on an 18th-century Japanese palanquin. As one-third of the lacquer on the pole was missing, the polyvinyl alcohol fill worked well to fill large areas quickly and efficiently. At present, 8 years since treatment, the fills remain unchanged (fig. 2).
Fig. 2.
Detail of the Japanese palanquin pole with polyvinyl alcohol and calcium carbonate fills, before inpainting
 |
This method has also been used with success by Jackson for infills on Chinese lacquerware from the Warring States period (Jackson and Watson 1995).
2.6 EPOXY RESIN
In general, because they are insoluble, epoxies are not recommended for lacquer, but in certain circumstances Milliput, a two-part filled epoxy, has been used successfully. Because Milliput can be shaped wet using molding tools, a very smooth surface can be obtained without sanding. This procedure reduces the danger of abrading the adjacent lacquer surface when smoothing the fill. In describing her method for filling a smooth lacquer screen, Jaeschke (1993) reports she used 20% Paraloid B-72 as a barrier to ensure that the fill would be reversible.
Neuman used Milliput to fill losses on a modern sculpture consisting of nine giant lacquered wooden links of chain (Neuman and Martin 1996). In this case, not only was the avoidance of abrasion a consideration, but the fills would be subjected to a great deal of stress during display. A softer fill material such as polyvinyl alcohol would have been completely unsuitable.
Often the hinges on heavy Chinese screens have been ripped out or loosened through improper handling or extended use. Epoxy resin mixed with an equal amount of glass microballoons is very useful for filling these enlarged holes. The epoxy resin provides the necessary strength to allow the reattaching of the hinges in the same position as in the original, and the final surface finish may be carried out using another method.
In general epoxy is not the first material a conservator would consider for filling lacquer. Its poor aging characteristics and lack of reversibility are valid reasons for rejecting it. However, there may be circumstances, as described here, in which it would be considered acceptable.
2.7 PARALOID B-72 AND MICROBALLOONS
As the surface gloss of Paraloid B-72 is quite unlike lacquer, it is not used as fill material on its own. It has, however, been used successfully bulked with glass microballoons as a fill to support tented lacquer. When an organic substrate, usually wood, has permanently shrunk and the surface layers of lacquer no longer fit, the conservator must choose one of three treatment options. Part of the lacquer could be removed so the remaining lacquer will lie flat, or the lacquer could be adhered to the surface with an overlapping portion. The third option to prevent loss of design or original material is to support the tented lacquer in its distorted position.
At the Royal Ontario Museum tests were performed to find a suitable material to support tented areas of lacquer. A combination of Paraloid B-72 and glass microballoons seemed to hold a lot of potential, as it could be injected through a syringe and would be strong enough to support the fragile lacquer surface. Paraloid B-72 was chosen due to its good aging characteristics and reversibility and because it can be dissolved in a number of solvents. Other resins might also be appropriate for use.
Tests were performed to find the appropriate formulation that would allow the resin and microballoons to flow under the lacquer, spread out evenly, adhere to the surface, and dry. These activities had to be carried out without affecting the lacquer surface and also be reversible in the future. The tests were carried out on strips of distorted 200-year-old lacquer that were no longer attached to an artifact. The strips were adhered to 4-ply mat board, leaving the distortions in place.
The Paraloid B-72 was dissolved in different solvents, then microballoons were added with approximately 1 part resin mixture to 2 parts microballoons by volume. The following combinations were tried: 50% B-72 in acetone/ethanol 1:1, 30% B-72 in xylene, 40% B-72 in acetone/ethanol 1:1, 10% Klucel G (hydroxypropyl cellulose) in ethanol, 15% B-72 in Super Hi-Flash (a petroleum distillate), 25% B-72 in acetone/ethanol, and 30% B-72 in Super Hi-Flash. The results of these mock-ups—subjective judgment based on appearance of the lacquer, ease of use, and drying time—indicated that the nonpolar solvents are the safest because they will not affect the lacquer layers. Unfortunately the toxicity and the long drying times sometimes makes them impractical for large objects. The combination of acetone and ethanol works well, but it will soften lacquer if it is exposed too long. This problem can be overcome by treating one small area at a time and allowing for thorough drying before proceeding to the next section. Of course, as with any method, tests should be carried out to ensure the mixture chosen will not affect the particular object.
These formulations with microballoons are also useful for deep cracks. For example, the author has used it on several late Chinese cabinets in which the wood had shrunk to such an extent that there were large gaps between the panels. In addition, polyvinyl acetate in acetone/ethanol with microballoons can also be used for filling these deep cracks. Air trapped in the mixture adds to the elasticity, making it flexible enough to accommodate small dimensional changes.
2.8 SURFACE FINISHES TO IMITATE LACQUER
With the exception of the wax and polyester fill, all of the above require separate matching of the surface. In the past, the author has tried many materials to imitate the surface of lacquer. It makes little difference to the top coat whether a traditional rabbit skin glue gesso or the polyvinyl alcohol fill is used. What is required is that the underfill be smoothed perfectly, as any imperfections may show up in the final product.
A number of materials have been tried as the top coat and immediately rejected. Paraloid B-72, for example, did not have the right gloss, and watercolors with varnish did not have the depth of color necessary. These methods work for small areas of inpainting but not for large areas where matching the color and luster is more difficult. In addition, methods requiring solvents were unsuitable for inpainting large objects where adequate ventilation was unavailable.
2.9 ACRYLIC EMULSIONS AND DISPERSIONS
Acrylic paints have been used for the past decade to imitate lacquer (Umney 1987). They clearly have many advantages, such as ease of use, numerous available colors, and no special ventilation requirements. In addition, the surface of the surrounding area can easily be matched by coating thin layers of gloss medium until the right luster is reached. Unfortunately there are also many disadvantages to acrylic paints. Most of the colors available are opaque and do not match the translucency of lacquer. To paint the acrylic smoothly, it has to be diluted to such an extent that the water may soften polyvinyl alcohol or gesso fills. Also, in this diluted state the paint loses most of its flow qualities and hiding power. Each subsequent layer increases the possibility of brush strokes showing, and since the final surface is very soft, it cannot be polished.
However, instead of paint, if one uses an acrylic emulsion that drys hard enough to be polished and one adds dye instead of pigment, the results can be impressive. Several years ago, a series of sample boards were created in order to try different materials that might prove useful. Rohm and Haas had several new water-based acrylics available, including Acrysol WS-24. A commercial water-based lacquer formulation, Mohawk Water Based Clear Lacquer is also available, although it must be used with ventilation.
Acrysol WS-24, an acrylic copolymer dispersion resin, seems to hold great promise for the museum conservator in imitating lacquer. It can be dyed with water-based aniline dye, and the surface can be polished to match the degree of gloss left on the original lacquer. It is easy to work with and readily reversible in alcohol or ammonium hydroxide (Rohm and Haas Co. 1983). But there are also a few disadvantages to Acrysol WS-24. The first is that it is a bit too reversible in alcohol. In a museum setting this is not a problem, but for objects that will be returned to private homes it may not be the best choice; an alcoholic beverage spilled accidentally on the surface will leave a mark. The second disadvantage is that there is some off-gassing of this material after drying. Oddly, tests done at the Royal Ontario Museum show that the vapor given off will tarnish silver in an enclosed space; therefore, it might not be suitable for imitating lacquer with silver decoration. As with all water-based materials, acrylic emulsions spilled on the surrounding area can leave marks on the surface of light-damaged lacquer. The high alkalinity of the emulsion accelerates this damage.
Mohawk Water Based Clear Lacquer is not as readily reversible in alcohol as Acrysol WS-24, so it is suitable for objects that will be handled. Because it has a pH of approximately 7, it is less likely to mark a light-damaged surface. Unfortunately Mohawk Water Based Clear Lacquer has not yet been tested for long-term stability. It can be used in exactly the same method as the WS-24 with two caveats. It does contain some solvent, so it must be used with ventilation, and a drop in temperature below 15°C during drying will result in a cloudy coating. Mohawk comes in two types, matte and glossy, but either can be used to match a finish by polishing.
The following is an example of the technique using acrylic paints to achieve the smooth look of a lacquer finish. To imitate the surface of lacquer on an 18th-century palanquin at the Royal Ontario Museum, Liquitex acrylic paint was selected because of its ease of use, in terms of time and health hazards (fig. 3). A transparent purple dye was added to the ivory black to give the paint some translucency, and three or four thin coats were applied. While this coating did not come close to imitating the effect of lacquer, it was an improvement over opaque colors. The goal of the decoration was to achieve the same effect as the maki-e (“sprinkled picture” in Japanese), so similar processes were followed. First, a red acrylic layer was applied, followed by a gold layer. These were then touched up to match the existing original in color and gloss. Mica-based pigments were mixed with acrylic gloss medium to imitate gold, since genuine gold was too expensive for these extensive fills. Not only does this mica- and titanium-dioxide-based pigment reflect light in a way that imitates gold, but it also has the added benefit of not tarnishing since there is no metal in the pigment.
Fig. 3.
Same area of palanquin pole as figure 2, now inpainted with Liquitex paints and Liquitex medium with mica-based pigments
 |
The following procedure can be used to imitate black or translucent lacquer using an acrylic emulsion such as Acrysol WS-24 or Mohawk Water Based Clear Lacquer. Apply a polyvinyl alcohol or gesso underfill, and smooth it to a level lower than the surrounding surface. Select an appropriate color of dye, mix it up with the minimum amount of water necessary to dissolve the dye, then strain it and mix it with the Acrysol WS-24. The color and amount of dye depend on the piece to be imitated, but generally the same depth of color should be achieved in three or four coats. Apply the acrylic with a soft brush, taking care to avoid air bubbles. As in applying shellac, do not go over the same area twice when it is wet. The surface drys to the touch in about 20 minutes and can be lightly sanded in a few hours. Apply approximately four layers until the color is right, then apply two coats of the clear WS-24 before the final sanding and polishing. The surface can be polished much like a shellac finish. Start with 600-grade lubricated sandpaper and increase to 1,200, then switch to tripoli powder followed by finer polishing powders until the same depth of gloss is reached as the surrounding original lacquer. Again Micro-Mesh cushioned abrasive cloths are useful for polishing without a medium. In general, liquid or paste polishing compounds are incompatible with the acrylic, as even Solvol Autosol dissolves the surface.
The author has also used these acrylics with Japanese silver and gold powders and sprinkles to imitate a Japanese nashiji ground. By choosing the right grade of nashiji or metal powders and matching the color of the translucent urushi finish, one can come very close to the original finish (fig. 4). Red lacquer can also be matched by first dyeing the Acrysol WS-24 to the color of liquid urushi, then adding vermilion pigment.
Fig. 4.
A comparison of Acrysol WS-24 (left), Mohawk Water Based Clear Lacquer (bottom), and shellac japanning (right) against urushi with nashiji and maki-e decoration. The size and amount of nashiji were different from the Japanese piece; however, one can see that the color and gloss come close to the original for the WS-24 and the Mohawk samples.
 |
2.10 OTHER COATINGS
Polycite and Cashew are two synthetic coatings produced by Saito and Company in Japan to imitate urushi. Literature from Saito (1989) states that “the main materials consist of the principal ingredients of lacquer, such as Urushiol, Laccol, Thitsiol, and a similar chain compound Catechol or derivatives of Phenol and these are compounded by special process with Trialkenyl Phenol derivatives.” The literature goes on to say that Polycite is easy to use, may be applied by brush or spray, and can be polished just like urushi. Another advantage is that it does not cause a skin reaction, as does natural lacquer.
Polycite and Cashew do indeed do a good job of imitating lacquer, as company literature states. The main drawback for conservators, however, is that they are not reversible resins: they are extremely difficult to remove. They do have potential if used over a reversible underlayer, such as polyvinyl alcohol or Paraloid B-72. They have extremely good hiding power, and a lacquerlike surface can be achieved with as little as two coats. Minor difficulties are that they require a long drying time, during which dust becomes a problem, and as the vehicle is a petroleum solvent, they require proper ventilation.
2.11 TRADITIONAL JAPANNING
Traditional japanning with seed lac or other natural spirit resins used in European lacquer still have a place in restoration work. After all, European lacquer was developed to imitate Asian lacquer in the first place. This method is useful for replicating a missing part. The drawback to using this method as the surface for a fill is the application of numerous coats to achieve the right finish. Sanding between coats risks damaging the surrounding urushi, and in addition the whole process is very time-consuming. The surface does not last very long, but soon develops its characteristic craquelure. Instructions for japanning can be found in historical texts such as Stalker and Parker's Treatise on Japanning and Varnishing ([1688] 1971) or Dossie's Handmaid to the Arts (1764). A little experimentation and practice are required to adapt these recipes to modern use.
2.12 CONCLUSION
All of the above materials offer possible solutions to the problem of imitating lacquer for infilling. The author has not found a single method that can be used in all circumstances. In a way it is unreasonable to expect one method to answer all needs. After all, many different grades of urushi combined with other materials were used to create the original. The acrylic emulsions hold the most promise, as they are good at recreating the look of the basic lacquer.
Because a suitable substitute for maki-e decoration has not been found, the author carried out further experiments with traditional maki-e decoration on top of acrylic fills. The urushi adhered nicely to the acrylic, yet the whole fill remains reversible. The combination of a reversible base with urushi used for the decorative layers may answer the objections some people have to urushi as a repair material.
3 FILLS FOR WESTERN LACQUER
3.1 CHARACTERISTICS TO BE CONSIDERED DURING TREATMENT
There are two types of Western lacquer—spirit varnishes and oil varnishes. Both have been known as japanning for at least 200 years. Spirit-based japanning appeared in Europe during the 16th century, while the oil finishes (often with copal resin added) were first developed as a coating for metal in the early 18th century. In the past these two types of japanning have often been mistaken, one for the other, sometimes with disastrous results. Most conservators have encountered examples of alligatored finishes in which an oil varnish has been mistakenly applied over the spirit-based resin surface. Treatment should take into account which type of lacquer has been used.
In no case is it appropriate to use urushi to fill losses in European japanning because they are radically different materials. Occasionally one finds examples of furniture in which Asian lacquer panels have been incorporated. As European materials are used in the construction of these composite objects, it is still inadvisable to use Asian lacquer for repairs. Many times the surface of the Asian lacquer has been recoated with varnish at the time the cabinet was constructed. Now part of an entirely new work of art, these panels can no longer be conserved as Asian objects.
Some fills for japanning are the same as those for urushi-based objects. In nearly all treatments the approach has been to treat the ground and the resin layers separately. For japanned finishes that were made using spirit varnishes, the main concern during conservation is that the solubility of any medium used should be different from the original surface. As these japanned finishes involved a great many natural resins, they often remain soluble for many years, even centuries. Successful treatments have utilized materials with an appearance similar to natural resin, but with different solubility. In general the spirit-based varnishes are not soluble in nonpolar solvents such as mineral spirits or xylene. For japanning that was originally done in a baked oil finish, which tends to be more insoluble, the choice of media and solvents is much greater. Nonetheless, solubility tests should always be carried out prior to commencing work.
3.2 GESSO
The grounds for spirit-based japanning are most often made of rabbit-skin glue or hide glue and whiting, but even contemporaneous literature debates the effectiveness of a ground. Robert Dossie states in the Handmaid to the arts (1764),
One principal variation in the manner of japanning is, the using or omitting any priming or undercoat on the work to be japanned…. There is nevertheless this inconvenience always attending the use of an undercoat, that the japan coats of varnish and color will be constantly liable to be cracked and peeled off by any violence, and will not endure near so long as the bodies japanned in the same manner, but without any such priming.
These observations continue to prove sound, as the frequent losses to this material demonstrate.
Since these objects were first fabricated, the losses have often been filled with the same material as the original: gesso. The disadvantage of this method is that fills would be difficult to remove without damage to the original. If traditional gesso is used, barium sulphate can be added so that at least the fills will be readily apparent when x-radiographed.
In making gesso fills there are a number of cautions. In friable areas it goes without saying that the surrounding area is first consolidated. The original surface surrounding the losses should be protected from the gesso and subsequent sanding with a removable varnish. Due to the high water content, one must take care when applying the gesso not to soak the substrate. A dough is preferable to many layers of liquid gesso, as would be applied in gilding. Since gesso fills shrink on drying, several applications are necessary.
Depending on the circumstances, one might want to vary the strength of the rabbit skin glue considerably. Ballardie (1994) described the use of a very weak pigmented gesso to fill shallow losses in varnish layers of a japanned cabinet prior to cleaning. In this particular case the gesso was strong enough to support the surrounding fragile japanning, yet easily removed as it was not in direct contact with the original ground.
An English japanned clock case with a casein ground was treated by Bigelow (1990). Here a 10% rabbit-skin glue and whiting gesso was used as a reversible infill for losses to the ground only. Japanning layers were infilled with different materials.
A traditional approach does not always need to be used. For a gesso ground or one with similar properties, polyvinyl alcohol and whiting can also be used, as outlined in the urushi section of this article. On a late 17th-century cabinet in the Royal Ontario Museum Collection many of the raised decorations were lost or crumbling. After consolidation, the losses were infilled with 6% polyvinyl alcohol in water, whiting, and dry pigments (Webb 1997).
3.3 PAPIER-MÂCHÉ
Eighteenth- and 19th-century European and American manufacturers took advantage of new methods to produce hard paper boards for japanning. Various oil formulations, usually consisting of boiled linseed oil, burnt umber, red lead, and often asphaltum were applied directly to the dried boards, then stoved to dry the coating (Dossie 1764). A ground layer was not used in this method. If a gesso ground is found, it suggests that the object was produced by other means.
Losses to this material usually involve the paper substrate as well as the lacquer layers. As the oil varnish and the papier-mâché are such different materials, it is advisable to treat these two layers separately.
At the Royal Ontario Museum, the simple method of building up layers of paper and methyl cellulose has been used with success. Good quality Japanese paper was used, and each layer was allowed to dry completely before the next was applied. Fills on a sewing table done with this method appear unchanged after 10 years (fig. 5).
Fig. 5.
An infill on papier-mâché using Japanese tissue and wheat starch paste built in layers
 |
Other conservators have found that the preparation of papier-mâché panels in a method similar to the original works well. Van der Reyden and Williams (1986) have outlined a method involving taking a mold of an intact area similar to the area of loss. High-quality oriental paper coated with wheat starch paste is pressed into the mold and baked at 100°F. The baked paper can be carved to its final shape, then adhered into place with wheat starch paste. In both examples the japanned surface area was imitated using different materials.
3.4 WAX
Although it has been used in the past (Moir 1979), for the most part the author would avoid wax formulations where there are losses of the paper substrate or a gesso ground. As with urushi, the use of a wax as a fill makes it extremely difficult to carry out repairs using other materials. Beeswax, carnauba, or microcrystalline wax formulations such as those given in the urushi section of this article could be used for fills that involve only the surface layer.
Often many japanned pieces of furniture include raised areas that were applied after the basic japanning was complete. The original use of gesso and other incompatible materials over the varnish contributes to their frequent loss. Wax has been used successfully to recreate or fill these losses. In this case the wax is sitting on top of the original japanned surface, as are the raised areas of the original. Hill (1976) describes the use of microcrystalline wax, rottenstone, and pigment for this purpose on the Pimm highboy.
3.5 PARALOID B-72 AND MICROBALLOONS
The author has also experimented with the use of 25% Paraloid B-72 or B-67 bulked with a small amount of the finest grade of glass microballoons and black pigment to fill small losses. This formula works well for the losses around mother-of-pearl decoration, and for a larger area it should also be very successful.
3.6 IMITATION OF SURFACE LAYER
3.6.1 OIL PAINTS
Oil paints on japanning have been used extensively in the past, but they have disadvantages. Besides being irreversible, they can accelerate deterioration when applied over a spirit varnish. As the oil continues to dry and shrink, it pulls the japanning off of the surface. Although more recently oil paints have been used over a separating layer of wax or Paraloid B-72 (Beale 1994), the author is still wary of their use .
3.6.2 ACRYLICS
On japanned finishes that were made using spirit varnishes, the main concern is that any inpainting medium should be soluble in a solvent different from that for the original surface. Successful treatments have utilized materials with an appearance similar to natural resin but that dissolve in different materials. For this reason the acrylic emulsions that were suggested for use with Asian lacquer are not always suitable for this type of japanning.
For japanning that was originally done in a baked oil finish, the choice of inpainting media is much greater. Here acrylic paints such as Liquitex are again suitable.
For both types of japanning, Paraloid B-67 or B-72 can be mixed with dye to achieve a good approximation of the aged varnishes. Orasol dyes by Ciba-Geigy are particularly useful for this purpose. These dyed resins can be applied in layers over a ground of traditional gesso, acrylic gesso, or polyvinyl alcohol and whiting to build up the fills to surface level. Either synthetic resin can be used, but the gloss of Paraloid B-67 is more similar to the original japanned surface. Bigelow (1990) has described the use of Paraloid B-72 mixed with dry pigment to inpaint areas on a clock case with opaque japanned surfaces. A similar clock conserved by Park (1994) utilized the same method with Paraloid B-67 but with added microcrystalline wax to give a sheen similar to the japanned surface.
For the most part the author's inpainting is done in an acrylic medium such as Liquitex following the application of a barrier coat. Losses in gilding can be imitated well using gloss medium and Afflair Lustre pigments (mica-based). Other media such as Paraloid B-72, B-67, or PVA AYAF and dry pigments in a standard inpainting approach have also been used to imitate the surface successfully (figs. 6, 7).
Fig. 6.
English papier mâché sewing table showing Japanese paper infill before inpainting
 |
Fig. 7.
Same infill as in figure 6 after inpainting with Liquitex paints and Liquitex medium with micabased pigments
 |
3.7 OTHER METHODS
Bruno (1996), working on a Mexican lacquer tray, used an interesting technique developed at the Freer Gallery of Art. This technique used Parafilm M, an American Can Company product that the Canadian Conservation Institute tested and found to be a blend of polyethylene and polyisobutylene. An isolating layer of Paraloid B-72 was applied to the loss prior to trimming the Parafilm to shape. Then, with a heated spatula and silicone release paper, layers of parafilm were built up to the level of the original surface. The excess was trimmed away with a scalpel. Inpainting, to match the surrounding opaque surface, was done using Liquitex acrylics. An advantage of this method is that the fill is particularly easy to reverse; unfortunately, the Parafilm does not work well for imitating translucent layers.
3.8 VARNISHES
Often japanned furniture is revarnished to help integrate the fills into the overall appearance of the object. Over the centuries revarnishing has often resulted in an accumulation of dark yellow and brown layers. Even the use of synthetic resins can have problems. While Paraloid B-72 can be dissolved in many solvents that are different from solvents that work for the original, its appearance is very unnatural and has given several pieces of japanned furniture a look of “plastic.”
Occasionally the author has used a synthetic resin in a very thin coat but remains convinced that it does not have the rich luster of true japanning. The final result was disappointing. This overall varnishing of japanned furniture should be avoided if possible. Satisfactory, but not always invisible, fills can be achieved using the methods outlined above.
3.9 TRADITIONAL JAPANNING
The use of traditional japanning to repair small losses might make it difficult to differentiate from the original and to reverse the fill in future years. Traditional japanning, however, may be the best option for replacing missing parts or large isolated areas of a piece of furniture.
The difficulty in reproducing the original finish arises in determining exactly what methods and materials were used. Even a cursory look at the contemporary literature will demonstrate the complicated nature of these finishes. However, with chemical analysis of the existing japanning and a thorough understanding of the original formulas, good quality japanning can be reproduced today.
Walch (1993) outlined her investigations of several methods used in the past. Her research and the analysis done by Koller (1993) have contributed to the understanding of the numerous resins used in these formulations. Their work on the Munich Residenz cabinet revealed that what looked like a simple red japan was, in fact, quite complicated (Walch et al. 1996). Synthetic cinnabar was applied to the wood in a seed lac preparation, followed by layers of a more complicated translucent varnish composed of sandarac, larch turpentine resin, mastic, and camphor. The addition of lake cochineal and cochineal dye to final layers of the original enhanced the red color in a cost-effective manner. The lost panels of the Munich Residenz cabinet have now been recreated using the technique discovered through this research.
3.10 CONCLUSIONS
To develop new materials and methods of fills that are visually compatible with either type of japanning, understanding the original processes is paramount. Through analysis, examining texts, and reproducing original recipes, we come to the realization that often the method of application is as important as the materials used. With an improved understanding of technique we will be able to develop better fills in the future.
REFERENCES
Arai, H.1993. The restoration of Japanese urushi objects in Europe: Museo d'Arte Orientale in Venezia. Conservation of Urushi Objects. Tokyo: Tokyo National Research Institute of Cultural Properties. 115.
Ballardie, M.1994. Conservation of an 18th century chest lacquered and japanned. Lacquerwork and japanning: Postprints of the United Kingdom Institute for Conservation conference. London: UKIC. 11–13.
Beale, R.1994. Restoration of a late 17th century japanned longcase clock. Lacquerwork and japanning: Postprints of the United Kingdom Institute for Conservation conference. London: UKIC. 45–50.
Bigelow, D.1990. A review of the consolidation system used in the conservation of a japanned clock. Wooden Artifacts Specialty Group postprints, American Institute for Conservation 18th Annual Meeting, Richmond, Va. Washington, D.C.: AIC. N.p.
Bruno, L.1996. Conservation record of Batea(tray). New York: Brooklyn Museum.
Chase, W.T.1988. Lacquer examination and treatment at the Freer Gallery of Art: Some case histories—urushi. In Urushi: Proceedings of the 1985 urushi study group, ed.N. S.Brommelle and P.Smith. Los Angeles: Getty Conservation Institute. 95–112.
Derrick, M., C.Druzik, and F.Preusser. 1988. FTIR analysis of authentic and simulated black lacquer finishes on eighteenth century furniture. In Urushi: Proceedings of the 1985 urushi study group, ed.N. S.Brommelle and P.Smith. Los Angeles: Getty Conservation Institute. 227–34.
Dossie, Robert. 1764. The handmaid to the arts. 2d ed.London: J. Nourse. 481, 493.
Hebrard, M., and S.Small. 1991. Experiments in the use of polyvinyl alcohol as a substitute for animal glues in the conservation of gilded wood. In Gilded wood conservation and history, ed.R.Bigelow, E.Cornu, P.Landrey, and C.VanHorne. Madison, Conn.: Sound View Press. 277–90.
Hill, J. H.1976. The history and technique of japanning and the restoration of the Pimm highboy. American Art Journal (November): 82.
Jackson, T.1994. Conservation and restoration of a 13th century lacquer dish from the Song Period. Lacquerwork and japanning: Postprints of the United Kingdom Institute for Conservation conference. London: UKIC. 36–38.
Jackson, T., and J.Watson. 1995. The conservation of waterlogged Chinese lacquerware from the warring states period. Conservator19:45–51.
Jaeschke, H.1993. Two approaches to gapfilling Oriental lacquer. Newsletter of the Interim Working Group on Lacquer of the International Council of Museums Committee for Conservation3(May):13.
Jaeschke, H.1994. Examination of lacquer for conservation. Lacquerwork and japanning: Postprints of the United Kingdom Institute for Conservation conference. London: UKIC. 6–10.
Kitamura, K.1988. Some thoughts about conserving urushi arts objects in Japan, and an example of conservation work. In Urushi: Proceedings of the 1985 urushi study group, ed.N. S.Brommelle and P.Smith. 113–20.
Koller, J.1993. The scientific analysis of Western coatings systematic approach and case studies. Conservation of urushi objects: Postprints of the international symposium on the conservation and restoration of cultural property. Tokyo: Tokyo National Research Institute of Cultural Properties. 241.
Konishi, T.1993. Conservation of urushi cultural artifacts: Conservation, intervention, and restoration of urushiware. Conservation of urushi objects: Postprints of the international symposium on the conservation and restoration of cultural property. Tokyo: Tokyo National Research Institute of Cultural Properties. 91–113.
Moir, G.1979. The care of papier-mâché. OMA Quarterly, (Summer): 19–20.
Murose, K.1996. On ryukyu urushi technique and restoration. Working group on furniture and lacquer: ICOM Committee for Conservation preprints, 11th Triennial Meeting, Edinburgh, Scotland. London: James and James. 915–19.
Nakajima, T.1988. Conservation of Chinese urushi: Methods and difficulties. In Urushi: Proceedings of the 1985 urushi study group, ed.N. S.Brommelle and P.Smith. Los Angeles: Getty Conservation Institute. 87–89.
Neuman, I., and J. S.Martin. 1996. Where East meets West: The conservation of a modern, large-scale, black lacquer sculpture exhibited in a public space. Objects Specialty Group postprints. American Institute for Conservation of Historic and Artistic Works 25th Annual Meeting, Norfolk, Va. Washington, D.C.: AIC. 42–61.
Norman, J., and S.Koob. 1994. Attention to lacquer at the Freer Gallery of Art and the Arthur M. Sackler Gallery. Newsletter of the Interim Working Group on Lacquer of the ICOM Committee for Conservation (February): 5–6.
Onodera, H.1982. Repair of wooden sculpture: The conservation of wooden objects. Postprints of the international symposium on the conservation and restoration of cultural property, 1982. Tokyo: Tokyo National Research Institute of Cultural Properties. 147–56.
Park, J.1994. Conservation principles applied to a restoration project: The Allam clock case. Lacquerwork and japanning: Postprints of the United Kingdom Institute for Conservation conference, 1994. London: UKIC. 41–44.
Piert-Borgers, B.1993. Aspects and problems of the application of urushi in the restoration of objects from European collections. Conservation of urushi objects: Postprints of the international symposium on the conservation and restoration of cultural property, 1993. Tokyo: Tokyo National Research Institute of Cultural Properties. 147–65.
Rohm and Haas Co. 1983. Acrysol WS-24 Acrylic copolymer dispersion resin. Company brochure. Philadelphia: Rohm and Haas Co.
Saito and Company Ltd. 1989. Polycite is superior to natural lacquer. Company brochure. Osaka, Japan: Saito and Co. Ltd.
Simonov, V.1990. The method for the conservation treatment of the Vietnamese lacquer sculpture Donatur. ICOM Committee for Conservation preprints, 9th Triennial Meeting, Dresden. Paris: ICOM. 658.
Simonov, V.1996. Method of Coromandel lacquer conservation. Paper presented at the Committee for Conservation, ICOM, 11th Triennial Meeting, Edinburgh, Scotland.
Stalker, J., and G.Parker. [1688] 1971. A treatise of japanning and varnishing. Reprint, London: Alec Tiranti.
Thornton, J.1991. The use of non traditional gilding methods and materials in conservation. In Gilded wood conservation and history. Madison, Conn.: Sound View Press. 220.
Umney, N.1987. Oriental lacquers. Part 2, Conservation News no. 33 (July).
van derReyden, D., and D. C.Williams. 1986. The technology and conservation treatment of a nineteenth century english “papier mâché” chair. AIC preprints, American Institute for Conservation 14th Annual Meeting, Chicago. Washington, D.C.: AIC. 125–42.
Walch, K.1993. Traditional coating techniques in Germany: General overview and conservation case studies. Conservation of urushi objects: Postprints of the international symposium on the conservation and restoration of cultural property. Tokyo: Tokyo National Research Institute of Cultural Properties. 225–39.
Walch, K., J.Koller, U.Baumer, and C.Fischer. 1996. The red lacquer-work in the cabinet of miniatures in the Munich Residenz. ICOM Committee for Conservation preprints, 11th Triennial Meeting, Edinburgh, Scotland. London: James and James. 920–22.
Webb, M.1994. An examination of fill materials for use with lacquer objects. Lacquerwork and japanning: Postprints of the United Kingdom Insitute of Conservation conference. London: UKIC. 30–35.
Webb, M.Forthcoming. Four japanned cabinets: A variety of techniques. Postprints of painted wood: History and conservation. Los Angeles: Getty Conservation Institute.
Yamashita, Y.1995. Thoughts on the conservation of urushi cultural properties: The conservation of the “Shinobukuzu Raden makie San-e Bako.” Newsletter of the Furniture and Lacquer Working Group of ICOM Committee for Conservation (April):15.
SOURCES FOR MATERIALSAcrysol WS-24Rohm and Haas, Independent Mall West, Philadelphia, Pa. 19105 Afflair Lustre pigmentsEM Industries, Inc., 7 Skyline Dr., Hawthorne, N.Y. 10532, (914) 592–4660 Micromesh cushioned abrasive clothsMicro-surface Finishing Products, Inc., 1217 W. Third St. (or Box 818), Wilton, IA 52778 MilliputMilliput Corp., Unit 5, the Marion, Dolgellau, Mid Wales LL40 1UU, U.K. Mohawk Water Based Clear LacquerRohm and Haas, Independent Mall West, Philadelphia, Pa. 19105 Orasol dyesCiba-Geigy Corp., 7 Skyline Dr., Hawthorne, N.Y. 10532-2188 Parafilm MLaboratory supply companies Paraloid B-72Rohm and Hass Co., Independent Mall West, Philadelphia, Pa. 19105
AUTHOR INFORMATION
MARIANNE WEBB completed her B.A. in fine art at the University of Toronto in 1976. She graduated from the Art Conservation Programme at Sir Sandford Fleming College in 1982. Since then she has been the decorative arts conservator at the Royal Ontario Museum. She specializes in organic and mixed materials with a particular interest in both oriental and European lacquer and has lectured widely on the subject. She is presently the coordinator of the ICOM Committee for Conservation Working Group on Lacquer. Address: Royal Ontario Museum, 100 Queen's Park, Toronto, Ontario, Canada M5S 2C6.