ANTIFUNGAL PROTECTION AND SIZING OF PAPER WITH CHITOSAN SALTS AND CELLULOSE ETHERS. PART 1, PHYSICAL EFFECTS
MARIA DEL PILAR PONCE-JIMÉNEZ, FERNANDO A. LÓPEZ-DELLAMARY TORAL, & EZEQUIEL DELGADO FORNUÉ
4 RESULTS
4.1 VISCOSITY AND PH OF THE POLYMERIC SOLUTIONS
The viscosity of 2% solutions of chitosan is very low in comparison with cellulose ethers, thus facilitating the penetration of the solution into the paper fiber mat and making impregnation more homogeneous. All of the chitosan solutions were acidic (table 1) as a result of the preparation method of the solutions and not from any inherent characteristic of the chitosan.
MC and HPMC were also acidic but could be easily adjusted by adding any alkaline agent, such as calcium hydroxide (Ca [OH]2). On the other hand, chitosan solutions will precipitate at a pH higher than 5.8.
Table .
Determination of Viscosity and pH of Solutions (2% w/v) Employed as Sizing Agents and Protective Coatings on Whatman No. 1 Filter Paper
 |
4.2 EFFECTS OF THE COATINGS ON PHYSICAL AND MECHANICAL PROPERTIES OF THE PAPER
Before the antifungal protection tests (Ponce-Jiménez et al. 2002), the physical and mechanical properties—folding endurance, zero-span tensile strength, brightness, and pH—were evaluated to determine how the coating affected these properties of paper.
Treatment with chitosan increased both the paper's zero-span tensile strength and its folding endurance. Treatment with cellulose ethers had the same effect, but to an even greater degree (figs. 2, 3). Sterilization with EtO slightly increased the zerospan tensile strength in all cases.
Folding endurance increased significantly with both treatments, although cellulose ethers were more effective than chitosan. On the other hand, after sterilization with EtO, the folding endurance decreased in all treated papers, but more so in the cellulose ether–treated samples (see fig. 3).
Fig. 2.
Graph of zero-span tensile strength, sterilized and unsterilized samples. Results are given in newtons. The bars indicate the mean, and each bar shows the standard deviation (SD) of eight replicas. The tests were done with a pendulum-type tester (TAPPI standard T231 cm-85, TAPPI 1985) after a period of conditioning at 50% ± 2% RH and 23 ± 1°C (TAPPI standard T402 om-93, TAPPI 1993).
 |
The resulting percentages of brightness before and after sterilization with EtO are shown in table 2. The last column indicates the difference between the means of the first and the second column.
Chitosan salts caused more loss of paper brightness than cellulose ethers did. The sterilization with EtO slightly darkened the paper coated with either chitosan salts or cellulose ethers.
The pH and viscosity using the three chitosan salts were very similar (see table 1). Cellulose ethers produced higher viscosity than the chitosan salts, and the pH was variable.
Table 3 shows the results of the pH measurements of the aqueous extracts of paper before and after the sterilization with EtO.
Fig. 3.
Results of folding endurance on samples of Whatman no. 1 filter paper, before and after sterilization with ethylene oxide. Units are given in number of double foldings. Bars indicate the mean, and each bar shows the standard deviation (SD) of eight replicas. Tests were done with a Schooper tester (TAPPI standard T423 om-89, TAPPI 1989) after a period of conditioning at 50% ± 2% RH and 23 ± 1ºC (TAPPI standard T402 om-93, TAPPI 1993).
 |
Table .
Percentage of Brightness in Samples of Whatman Paper No. 1 Treated with Different Types of Coatings, before and after Sterilization with EtO
 |
Table .
Results of pH Determination of the Aqueous Extracts of Paper, before and after Sterilization with Ethylene Oxide
 |
Chitosan salt solutions are more acidic than cellulose ether solutions. Sterilization with EtO caused a slight decrease in the pH of all the samples.
|