Subject: Edison phonograph cylinders
Sue Dunlap <sdunlap [at] ACS__WOOSTER__EDU> writes >A fellow employee asked me how to safely remove mold from old Edison >phonograph cylinders made out of wax. In the early 70's I carried out a project which involved, prior to transcription, cleaning over 3000 wax cylinders, most of which had fungal growth on them. The same technique (and the equipment I built) were then used by the Library of Congress (for 9000+ cylinders) and the Archives of Traditional Music at Indiana University (for 7000+ cylinders). This cleaning process was quite simple and extremely effective: 1. Mix a tepid solution of Labtone Detergent (a proprietary formulation from VWR Scientific) until the mixture feels slippery (about 1% or so). Use deionized water to mix. 2. Immerse each cylinder in the solution while holding it with spread fingers inserted into the interior only. 3. Saturate a small (3x6") piece of polyester velvet or velveteen in the solution and while the cylinder is immersed, gently drag the velveteen around the cylinder's circumference, allowing the pile of the velveteen to gently "scrub" the grooves. 4. Rinse the cylinder thoroughly in running deionized water and stand on-end to dry on an absorbent or drained surface. The remaining water will bead on the surface and may be removed with "Webril Wipes" or similar non-abrasive cotton wipers (used for cleaning copier machine drums). The reason that I specify Labtone is that it is a balanced detergent that is formulated to effectively remove organic gunk and oily material. It is very effective on removing the fungal mycelium but doesn't harm the wax. It rinses off completely, leaving no residue. This detergent is intended for hand washing, so it doesn't destroy your skin although you will probably want to wear surgical gloves to protect the cylinders from skin oils. Although I have tested a broad range of other formulated laboratory detergents and individual detergent agents, none seems to perform as well as Labtone for this application. Avoid returning cleaned cylinders to the original packing. Discard any wool, cotton, glassine or felt liners in the cylinder boxes (they are actually pasteboard tubes) and insert new liners of 2-3 smoothly fitted layers of polyester felt. Cylinder boxes should be ventilated to avoid further fungal growth and often have a hole in the bottom which serves this purpose. If no hole is present, it might be a good idea to cut a 1" diameter hole in the box bottom. Alternatively, the Library of Congress had developed a nifty telescoping archival cylinder box that supports the cylinder from the inside on pyramid-shaped projections. They may still have these available and might be willing to sell a few. If you need more info or are interested in transcribing the cylinders, please contact me and I will be happy to give you some guidelines and refer you to people who have equipment for safe transcription. Geoffrey Brown Curator of Conservation Kelsey Museum University of Michigan Ann Arbor, MI 48109-1390 313-647-0439 *** Conservation DistList Instance 10:41 Distributed: Wednesday, October 23, 1996 Message Id: cdl-10-41-002 ***Received on Tuesday, 22 October, 1996
URL: http://cool.conservation-us.org/byform/mailing-lists/cdl/1996/1038.html
Timestamp: Monday, 16-Nov-2009 16:15:18 PST
Retrieved: Monday, 23-Nov-2009 14:21:44 GMT